Dependence of the Structural and Magnetic Properties on the Growth Sequence in Heterostructures Designed by YbFeO3 and BaFe12O19

1
Institute for Photon Science and Synchrotron Radiation, Karlsruhe Institute of Technology, Hermann-von-Helmholtz-Platz 1, D-76344 Eggenstein-Leopoldshafen, Germany
2
Laboratory for Electron Microscopy, Karlsruhe Institute of Technology, Engesserstr. 7, D-76131 Karlsruhe, Germany
3
Institute of Nanotechnology, Karlsruhe Institute of Technology (KIT), Hermann-von-Helmholtz-Platz 1, D-76344 Eggenstein-Leopoldshafen, Germany
4
Karlsruhe Nano Micro Facility, Karlsruhe Institute of Technology (KIT), Hermann-von-Helmholtz-Platz 1, D-76344 Eggenstein-Leopoldshafen, Germany
5
Department of Condensed Matter Physics, Charles University, Ke Karlovu 5, 121 16 Prague, Czech Republic
6
Institute for Applied Materials, Karlsruhe Institute of Technology, Hermann-von-Helmholtz-Platz 1, D-76344 Eggenstein-Leopoldshafen, Germany
7
Laboratory for Applications of Synchrotron Radiation, Karlsruhe Institute of Technology, Kaiserstr. 12, D-76131 Karlsruhe, Germany
*
Author to whom correspondence should be addressed.
Submission received: 8 March 2024 / Revised: 12 April 2024 / Accepted: 13 April 2024 / Published: 18 April 2024

Abstract

:
The structure and the chemical composition of individual layers as well as of interfaces belonging to the two heterostructures M1 (BaFe12O19/YbFeO3/YSZ) and M2 (YbFeO3/BaFe12O19/YSZ) grown by pulsed laser deposition on yttria-stabilized zirconia (YSZ) substrates are deeply characterized by using a combination of methods such as high-resolution X-ray diffraction, transmission electron microscopy (TEM), and atomic-resolution scanning TEM with energy-dispersive X-ray spectroscopy. The temperature-dependent magnetic properties demonstrate two distinct heterostructures with different coercivity, anisotropy fields, and first anisotropy constants, which are related to the defect concentrations within the individual layers and to the degree of intermixing at the interface. The heterostructure with the stacking order BaFe12O19/YbFeO3, i.e., M1, exhibits a distinctive interface without any chemical intermixture, while an Fe-rich crystalline phase is observed in M2 both in atomic-resolution EDX maps and in mass density profiles. Additionally, M1 shows high c-axis orientation, which induces a higher anisotropy constant K1 as well as a larger coercivity due to a high number of phase boundaries. Despite the existence of a canted antiferromagnetic/ferromagnetic combination (T < 140 K), both heterostructures M1 and M2 do not reveal any detectable exchange bias at T = 50 K. Additionally, compressive residual strain on the BaM layer is found to be suppressing the ferromagnetism, thus reducing the Curie temperature (Tc) in the case of M1. These findings suggest that M1 (BaFe12O19/YbFeO3/YSZ) is suitable for magnetic storage applications.

Graphical Abstract

1. Introduction

Different devices were recently produced by combining barium ferrite BaFe12O19 (BaM) with ferroelectric materials to form multiferroic systems with magneto-electric coupling at the well-defined and characterized interface in terms of sharpness, atomic step, and chemical interdiffusion. It has covered thin-film heterostructures such as SrBa2Ta2O9/BaM [1,2], Ba2EuFeNb4O15/BaM [3,4], multilayers composed of BaM layers with Pb(Zr,Ti)O3 (PZT) [5] or (Ba,Sr)TiO3 (BST) [6,7,8] or BaTiO3 perovskite layers [9], and multiferroic composites [10,11,12]. BaM is a very attractive material due to the high anisotropy Ha and coercivity HC fields [13,14], which are beneficial for obtaining performant film in perpendicular recording media. h-YbFeO3 belongs to the hexagonal rare earth ferrites h-(RFeO3) with R = Dy, where ferroelectricity and antiferromagnetism have been demonstrated at low temperatures [15]. Furthermore, room-temperature ferroelectricity has been confirmed for h-YbFeO3 grown on platinum Pt(111)/Al2O3(0001) [16] as well as for h-YbFeO3 grown by pulsed laser deposition on yttria-stabilized zirconia YSZ(111) [17,18]. The magnetic characterization of h-YbFeO3 was performed by measuring the polarization loops at different temperatures. Zero-field-cooled (ZFC) and field-cooled (FC) magnetic measurements demonstrated the existence of the magnetic transition Neel temperature of about 125 K [16,17,19]. Moreover, h-YbFeO3 has been demonstrated to possess a canted antiferromagnetic spin structure exhibiting a ferromagnetic moment [19]. There was an agreement about the existence of ferroelectricity and weak magnetic ordering in h-YbFeO3. Recently, there has been interest in building heterostructures based on h-YbFeO3. Xu et al. [20] designed a ferroelectric/dielectric bilayer structure with h-YbFeO3 as the improper ferroelectric (FE) and CoFe2O4 as the dielectric (DE) with the goal to tune the electrostatic energy of the (FE/DE) bilayer system and to study the electrostatic effect of the DE layer on the spontaneous polarization of the FE layer. Their atomic-resolution cross-sectional scanning transmission electron microscopy (STEM) high-angle annular dark-field (HAADF) imaging demonstrated a periodic arrangement with “two-up-one-down” and “two-down-one-up”, corresponding to the FE polarization [20,21,22]. The influence of the film thickness ratio of the FE to DE layers on the ferroelectric polarization has been discussed [21]. Heterojunction nanocomposites based on YbFeO3 were also successfully obtained by Tikhanova et al. [23] for application in photocatalysis, and a novel YbFeO3–BiFeO3 composite was synthesized by Chen et al. [24] for highly sensitive ppb-level acetone sensing at low temperatures. Zhang et al. [25] investigated the effect of the different interfaces on epitaxy and magnetism in h-RFeO3/Fe3O4/Al2O3 film (R = Lu, Yb) heterostructures. They demonstrated the enhancement of the magnetic remanence of the heterostructure h-RFeO3/Fe3O4/Al2O3 for temperatures below 50 K in comparison with the Fe3O4 layer. The degree of lattice misfit and the difference in the thermal expansion coefficient between individual layers play a relevant role in the growth of the heterostructure systems since they introduce microstructural strain and dislocations in the different layers. As a result, the film quality and the preferred growth orientation of YbFeO3 as well as its magneto-optical properties can be tailored by the choice of the substrate as it was demonstrated by Fu et al. [26]. This represents the most common approach used for altering the strain at the interface between the epitaxial film and the substrate and the resulting magnetic and electric properties [27,28]. Interfacial effects such as epitaxial strain [29], interface quality (i.e., defect, roughness, sharpness) [30,31,32], interdiffusion, and chemical intermixing [33,34] in multiferroic heterostructures have attracted tremendous attention for tuning and understanding the structure–property relationships as they allow one to control the magnetic interaction [35], spin ordering [36,37], and coupling across heterointerfaces, including ferromagnetic (FM)/antiferromagnetic (AFM) bilayer systems [30,32,33,34,35,36,37,38,39,40]. Several studies reported the occurrence of an exchange interaction based on the exchange bias (EB) at the interface of FM/AFM heterostructures. This phenomenon leads to a horizontal shift of the hysteresis loop with an enhanced coercive field HC when the magnetization loop is recorded at temperatures below the Neel temperature TN of the AFM after cooling the FM/AFM bilayers with an applied magnetic field. This was explained by pinning effects from uncompensated surface spins of the antiferromagnetic layer. However, in the case of a fully compensated AFM surface, where the AFM spins align themselves perpendicular to the FM spins to minimize the interfacial spin frustration, this resulted in a spin-flop coupling, which in return enhanced HC without inducing an EB. The investigation by Vafaee et al. [32] into La0.7Sr0.3MnO3/BiFeO3 (LSMO/BFO) heterostructures revealed the absence of an EB coupling for multistacks with a sharp interface, whereas a sizable EB coupling was observed for (LSMO/BFO) heterostructures with rough and chemically mixed interfaces [41,42,43,44,45,46,47]. Furthermore, the structural misfit at the heterointerfaces in other types of multifunctional heterostructures (e.g., BaFe12O19/BaTiO3 [9], La0.7Sr0.3MnO3/BiFeO3 [32], LaMnO3/LaFeO3 [33], LaMnO3/LaNiO3 [48]) was tuned by the material combination as well as by the growth sequence with the goal to modify the exchange interaction [9,32,33,48].
Temperature-dependent magnetic properties such as coercivity and zero-field cooling (ZFC) and field cooling (FC) were studied by Vafaee et al. [32] for La0.7Sr0.3MnO3/BiFeO3 (LSMO/BFO) heterostructures. In their investigation, they demonstrated that ZFC and FC curves were influenced by the stacking order of the layers. In a similar way, Chen et al. [33] also revealed that the temperature-dependent magnetization curves were affected by the growth sequences of the layer for LaMnO3/LaFeO3 heterostructures due to the difference in the chemical and structural qualities of the interfaces.
In our study, the FM order of BaM was combined with a canted AFM (CAFM) and ferroelectric order in YbFeO3 (YbFO) for two different growth sequences on yttria-stabilized zirconia substrates with (111) orientation, i.e., YSZ(111).
The structures of M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) were characterized by a combination of X-ray reflectivity (XRR), high-resolution X-ray diffraction (HRXRD), high-resolution transmission microscopy (HRTEM) as well as atomically resolved scanning STEM combined with energy-dispersive X-ray spectroscopy (EDXS). The goal of our study was to analyze the effect of growth sequences on the structure of the heterostructures M1 and M2 as well as on their resulting magnetic properties which were dependent upon temperature, basing this on the quality of the corresponding interfaces.

2. Experimental Section

2.1. PLD Growth of Multiferroic Heterostructure Systems

Two heterostructure systems named M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) were deposited by pulsed laser deposition with two different stacking orders on YSZ(111) substrates. The corresponding schematic presentation of the systems is given in Figure 1h,k. We used BaM and YbFeO3 targets with 99.9% purity and YSZ(111) with a miscut of αM ± 0.3° which was supplied from the company Surface, Germany (www.surfacenet.de). Prior to the growth, two pieces of YSZ(111) substrates which belonged to the same batch were cleaned with ethanol and isopropanol and annealed for 2 h under air in a furnace at 1200 °C. The individual BaM and YbFO layers in M1 and M2 were grown at Tg = 850 °C, with an oxygen pressure of P = 400 mbar, target–substrate distance Ts = 40 mm, and number of shots N = 10,000. Both M1 and M2 were grown with a laser frequency F of 1 Hz, an energy per pulse of 25 mJ (1.5 J/cm2), and a laser wavelength of 266 nm. The thicknesses for the BaM and YbFO layers which were grown under the above-mentioned conditions were approximatively ThBaMThYbFO ≅ 60 nm.

2.2. High-Resolution and X-ray Diffraction Reciprocal Space Mapping

A Rigaku SmartLab diffractometer, equipped with a 9 kW rotating X-ray tube, was used to conduct theta/2theta X-ray diffraction measurements. High-resolution parallel-beam geometry was used, using Cu Kα1 (λ = 1.540593 Å) radiation monochromatized with a Ge (220) 2-bounce monochromator. The measurements were taken with an incident slit width of 0.5 mm and two receiving slits, 0.5 mm and 1.0 mm wide, positioned in front of a scintillation detector.
Moreover, 2D-reciprocal space maps (2D-HRXRD) were recorded for the different BaM and YbFO reflections by using high-resolution diffraction at the NANO beamline at the KIT Light Source in Karlsruhe, Germany. All the 2D-HRXRD data of the symmetric and asymmetric reflections were measured using a Mythen linear detector positioned at the corresponding Bragg diffraction angles and by rocking the sample around the Bragg angle. All the X-ray measurements were performed at an energy E = 15 keV and a wavelength λ of 0.826 Å. Furthermore, azimuthal Phi(φ) scans were also measured by rotating the samples M1, M2, and BaM around the surface normal for the asymmetric reflections YbFO108 and BaM-1018.
The miscut was measured by using an Empyrean diffractometer. For the different azimuth angles in the range ϕ = [0–350°], the detector was positioned at the Bragg diffraction 2*QB of the symmetric YSZ111 reflection. We measured the deviation ΔQ = (Qmax − QB) from the rocking curve scan which corresponded to the (111) crystal lattice planes of the YSZ substrate, where Qmax is the angle of the diffraction peak maximum. The variation ΔQXRD derived from XRD as a function of the azimuthal angle ϕ is shown by red open circles in Figure S1a,b for M1 and M2, respectively.
For azimuthal angles ϕ equally space by 30° in the range of [0–350°], we measured the inclination of the sample surface in the reflectivity region where the detector was positioned at the exit angle corresponding to the specular reflections. The deviation of the incidence angle with respect to the exit angle gave ΔQXRR, which is plotted in blue open circles in Figure S1a,b for M1 and M2, respectively. The difference between the values of ΔQXRD(ϕ) and ΔQXRR(ϕ) for each azimuth value ϕ defined the angle between the film surface and the crystal lattice of the substrate in the given direction. These angles ΔQXRD(ϕ) and ΔQXRR(ϕ) were fitted by the function ΔQ(ϕ) = A × sin(ϕϕ0), and the amplitude A of the sine function was the miscut α of the substrate. The largest miscut αM = 0.67° was measured for the substrate of the sample M2, while for M1, it amounted to αM = 0.08°.
From the different 2D-HRXRD measurements, we derived the angular broadening of the diffraction profiles FWHMang for the symmetric reflections of BaM (BaM006, BaM0010, BaM0014, and BaM0016) and of YbFO (YbFO004, YbFO006, and YbFO008) to determine the degree α of misorientation and therefore to evaluate the quality of the BaM and YbFO layers for the M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) heterostructures. The X-ray data analysis included the determination of the peak positions, which corresponded to the maximum intensities, to derive the out-of-plane and the in-plane lattice parameters for the BaM and YbFO crystals. In addition, we calculated the residual strain and the lattice misfit between the individual layers in the M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) heterostructures. All the derived values are summarized in Table 1.
The lattice misfits fM1BaM/YbFO (resp. fM2YbFO/BaM) corresponded to M1 (resp. M2) between the BaM/YbFO (resp. YbFO/BaM) bilayers. Additionally, the lattice misfits fM1YbFO/YSZ (resp. fM2BaM/YSZ) between the substrate and the film interface YbFO/YSZ (resp. BaM/YSZ) were calculated as follows (see Table 1b). Moreover, the misfit between the substrate and the film was calculated by using the 3 × d( 11 2 ¯ )YSZ formula of the substrate to the a-parameter of the layers. This is because of the coincidence 3-to-1 in the lattice site between the substrate and the film.
f B a M / Y b F O M 1   [ % ] = a M 1 BaM a M 1 YbFO a M 1 YbFO × 100   and   f Y b F O / Y S Z M 1 [ % ] = a YbFO 3 d ( 11 2 ¯ ) YSZ 3 d ( 11 2 ¯ ) YSZ × 100  
f Y b F O / B a M M 2   [ % ] = a M 2 YbFO a M 2 BaM a M 2 BaM × 100   and   f B a M / Y S Z M 2 [ % ] = a M 1 BaM 3 d ( 11 2 ¯ ) YSZ 3 d ( 11 2 ¯ ) YSZ × 100  
where, the magnitudes aM1BaM, (resp. aM2BaM), aM1YbFO (resp. aM2YbFO), and d ( 11 2 ¯ ) YSZ are the in-plane lattice parameters of the BaM, YbFO, and YSZ substrates, respectively.
The in-plane residual strain (i.e., εM1YbFO// and εM2YbFO//) of the YbFO layer and (i.e., εM1BaM// and εM2BaM//) of the BaM layer was determined for the M1 and M2 heterostructures according to the following:
ε M 1 BaM / / = a M 1 B a M a B a M   F S   a B a M F S   and   ε M 1 YbFO / / = a M 1 Y b F O a Y b F O   F S   a Y b F O F S ,
ε M 2 BaM / / = a M 2 B a M a B a M   F S   a B a M F S   and   ε M 2 YbFO / / = a M 2 Y b F O a Y b F O   F S   a Y b F O F S .
The out-of-plane residual strain (εM1YbFO⊥, εM2YbFO⊥) of the YbFO layer and (εM1BaM⊥, εM2BaM⊥) of the BaM layer were calculated using the following formulas:
ε M 1 BaM = c M 1 B a M c B a M   F S   c B a M F S   and   ε M 1 YbFO = c M 1 Y b F O c Y b F O   F S   c Y b F O F S ,
ε M 2 BaM = c M 2 B a M c B a M   F S   c B a M F S   and   ε M 1 YbFO = c M 2 Y b F O c Y b F O   F S   c Y b F O F S .
a B a M   F S = 5.892   Å , c B a M   F S = 23.183   Å (ICSD 201654, space group P63/mmc) and a Y b F O   F S = 5.9652   Å , c Y b F O   F S = 11.7020   Å (ICSD 183152, space group P63 cm) correspond to the lattice parameters of the BaM and YbFO bulks in the free-standing (FS) states.

2.3. X-ray Reflectivity and Profile Density

The specular X-ray reflectivity (XRR) was measured by using a Rigaku Smartlab diffractometer. The data were measured using Cu-Kα1 radiation and a parallel beam with an X-ray mirror. The data were evaluated by the well-known method for the XRR analysis of multilayers with rough interfaces developed by Parratt [49]. The used model for fitting the XRR curves of M1 and M2 is described as following: a rough YSZ substrate, a thin interlayer between the substrate and the first layer, the first layer with rough interface, and a rough top layer. The fit was carried out by using a self-written script based on the least square fitting algorithm. All the fitting parameters are summarized in Table 2a.

2.4. Transmission Electron Microscopy

For the TEM inspection of the M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) heterostructure systems, cross-sectional specimens were prepared by focused ion beam (FIB) milling and by using an FEI Helios G4 dual-beam microscope. Prior to the FIB preparation, a thin gold layer was sputtered on the sample surface in order to reduce the damage of the heterostructures caused by the Ga+-ion bombardment. Subsequently, the standard FIB preparation of TEM lamellae was carried out, where first a Pt protection layer was deposited on top of the samples. Then, coarse FIB milling was carried out at a primary ion energy of 5 keV. The lamellae were attached to Cu lift-out grids and finally polished by a Ga+-ion beam with a low energy of 1 keV in order to minimize Ga+ implantation and material amorphization. The TEM investigations of M1 and M2 were carried out on two different transmission electron microscopes. An image-corrected 300 kV FEI Titan 80–300 microscope was used for the conventional TEM analysis of the layer structure (e.g., layer thickness, crystal structure). The crystal structure and microchemistry of the interfacial regions and the structure and composition of the BaM and YbFO layers were investigated in detail by a combination of STEM imaging and energy-dispersive X-ray spectroscopy (EDXS) with a probe-corrected Thermo Fisher Themis 300 microscope which operated at 300 kV and was equipped with a Super-X EDX detector. STEM images were taken by using a high-angle annular dark-field (HAADF) detector to obtain atomic number contrast. X-ray maps were recorded in STEM mode with typical measurement times of about 10 to 20 min, where a possible drift of the sample was automatically corrected by the cross-correlation of corresponding reference images. Using the Velox software package (Thermo Fisher Scientific, https://assets.thermofisher.cn/TFS-Assets/MSD/Datasheets/velox-datasheet.pdf, accessed on 12 April 2024), raw-data X-ray maps were quantified using the thin-film approximation after Cliff–Lorimer [50] in order to obtain element concentration maps and quantitative EDXS line profiles. Moreover, crystal structure information was obtained by a two-dimensional fast Fourier transformation (FFT) of the selected areas in atomically resolved STEM images.

2.5. Vibrating Sample Magnetometry

The magnetic in-plane (IP) and out-of-plane (OOP) magnetization loops were measured by using a VersaLab (San Diego, CA, USA) vibrating sample magnetometer from Quantum design with a magnetic field up to 2 Tesla and a sweeping rate (SR) of 10 Oe/s. There were two setups used for the magnetization measurements. For standard (OOP) and (IP) measurements, the standard mode of VSM was used which allows measurements from 50 K to 400 K. We measured the Curie temperature Tc of the M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) systems by recording the moment in-plane (IP) moment M// (H ⊥ to c-axis) during the heating process from 300 K up to 1000 K with a heating rate of 10 K/min in the VSM oven mode where the sample was wrapped by copper foil.
The measurements were performed for the M1(BaM/YbFO/YSZ), M2(YbFO/BaM/YSZ), and BaM (BaM/YSZ) systems at different temperatures T = 50, 70, 100, 120, 150, 200, 250, 300, and 400 K.
From the (IP) and (OOP) magnetization loops, the saturation magnetization Ms//(T), Ms(T), the remanent magnetization Mr//(T), Mr(T), the perpendicular and parallel squareness S(T) = Mr(T)/Ms(T) and S//(T) = Mr//(T)/Ms//(T), the out-of-plane and in-plane coercivity fields Hc(T) and Hc//(T), the coercivities ratio Rc(T)=Hc///Hc, and anisotropy field Ha(T) were derived. For more reliability, the anisotropy fields Ha(T) were determined using a more advanced approach where the effects of various factors on the shape of the magnetization reversal loop were considered as demonstrated by Zehner et al. [51]. The latter include the misalignment between the hard axis and direction of the applied magnetic field, the speed of sweeping as well as the domain structure and multiple magnetic phases. In this case, the average anisotropy fields Ha(T) were obtained for M1(BaM/YbFO/YSZ) and a (IP) hysteretic magnetization M2(YbFO/BaM/YSZ) from the crossing of extrapolating the linear part of curve to the saturation and saturation magnetization level of the (OOP) curves. This was applied for all hysteresis loops measured at different temperatures T = 50, 70, 100, 120, 150, 200, 250, 300, and 400 K. Zero-field cooling (ZFC) and field cooling (FC) where the M1 and M2 samples were cooled without and with applied fields H, respectively, were recorded in the temperature range from T = 50 to 400 K with an applied field H = 2000 Oe (H is parallel to the c-axis).

3. Results

3.1. Characterization of the Heterostructures M1 and M2

The diffraction patterns of M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ), which simultaneously comprise the reflections of the BaM, YbFO, and the YSZ substrates, are compared in Figure 1a. Moreover, 2D-HRXRD maps were also recorded for the BaM reflections BaM006, BaM008, BaM0012, and BaM0016 as well as for the YbFO reflections YbFO002, YbFO004, and YbFO008, but only the 2D-HRXRD data of YSZ222, YbFO008, and BaM0016 are presented in order to investigate the crystallographic orientation of the different layers with respect to each other in the out-of-plane direction (Figure 1f,g).
The presence of high reflection orders, namely BaM0016 and YbFO008, justifies the c-axis orientation for both samples, i.e., M1 and M2. The XRD pattern of sample M2 shows a higher background/higher diffuse scattering intensity than that of the M1 sample. Apart from the diffuse scattering, the lower intensity of the BaM0016 and YbFO008 reflections of the M2 sample also shows the poor crystal quality compared to M1. However, the quality of the individual layers cannot be distinguished due to the overlapping of reflection intensities. From 2D-HRXRD maps of symmetric and asymmetric reflections, we determined the lattice parameters of the BaM and YbFO layers in both heterostructures M1 and M2. We summarize them in Table 1. We found that the out-of-plane lattice parameter cM1BaM = 23.25 Å of the BaM layer in M1 is lower than that of the BaM layer in M2 (cM2BaM = 23.2942 Å) as it could be demonstrated by the diffraction peak shift of M2 towards lower diffraction angles (see Figure 1a). Furthermore, the cM1YbFO = 11.693 Å of the YbFO layer in M1 is slightly lower than the cM2YbFO = 11.715 Å of the YbFO layer of M2. This difference in the lattice parameters may be due to the variation in the chemical composition of the individual BaM and YbFO layers in the heterostructures M1 and M2, despite the similar employed PLD growth conditions.
Due to the change in the stacking order of BaM and YbFO in M1 and M2, the BaM layer interfaces with YbFO in M1 and with YSZ in M2, the misfit varies from fM1BaM/YbFO [%] = −3.56% in M1 to fM2BaM/YSZ [%] = −5.30% in M2. This leads to different in-plane lattice parameters (aM1BaM = 5.8151 ± 0.001 Å, aM2BaM =5.967 ± 0.001 Å) and therefore in-plane residual strain which changes from compressive εM1BaM// = −1.3% to tensile εM2BaM// = 1.3% (see Table 1c). The misfit at the interface BaM/YbFO in M1 is fM1BaM YbFO = −3.56%, while in M2, it is fM2YbFO/BaM = 0.35%. Due to the difference in the above-mentioned misfit values between M1 and M2 at the BaM interfaces, the in-plane residual strain changes from compressive to tensile, but the absolute value does not conspicuously alter. In turn, we do not expect a strong variation in the Curie temperature Tc between M1 and M2.
The YbFO layer interfaces with YSZ(111) in M1 and with BaM in M2, where the misfit varies from fM1YbFO/YSZ [%] = −4.42% in M1 to fM2YbFO/BaM [%] = 0.35% demonstrating a change from compressive to tensile. This has slightly affected the in-plane lattice parameters which vary from aM1YbFO = 6.0221 ± 0.001 Å to aM2YbFO = 5.9881 ± 0.001 Å and therefore decreases the in-plane residual strain from εM1YbFO// = 0.96% to εM2YbFO// = 0.39% (see Table 1b,c).
Figure 1b,c show the azimuthal Phi(φ) scans along the surface normal of the BaM-1018 and YbFO108 reflections for both samples M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ), respectively. Both layers show a 6-fold symmetry for both samples, indicated by the presence of reflections (each 60°). In Figure 1b, from the reflection intensities, it can be seen that the YbFO layer is 30°, rotated with respect to the BaM layer along the surface normal for sample M1, whereas in M2 (Figure 1c), the BaM and YbFO layers are well aligned with respect to each other. Therefore, the YbFO layer is rotated with respect to the underlayer in in-plane orientation. For the M1 and M2 heterostructures, the in-plane rotation relationship of the individual layers is visualized in Figure 1d,e by corresponding crystal structure models simulated along the [0001] direction.
The diffraction spots of BaM0016 and YbFO008 in Figure 1f are well aligned with respect to the YSZ222 diffraction spot along the qang direction for the M1 system, where the white dashed line crosses through the peak positions of the diffraction spots. This indicates that the c-axis of grown layers BaM and YbFO of M1 are well aligned with respect to the surface normal of the substrate YSZ(111). In the case of the system M2, BaM0016 and YbFeO008 diffraction spots show a clear horizontal shift in the qang direction with respect to the YSZ222 diffraction spot (see white dashed line in Figure 1g). This indicates the formation of an inclination angle β = 0.1° for M2(YbFO/BaM/YSZ) between the c-axes of the BaM and YbFO layers with respect to the normal of the YSZ(111) crystal planes. A more reliable determination of the true misalignment of the YbFO and BaM bilayers with respect to the YSZ(111) lattice planes normal would require comparing RSMs recorded for different azimuthal angles and fit sinusoidal functions similar to the miscut case.
In the case of M2, the HRTEM images of Figure S2c demonstrate the existence of steps at the substrate interface with an atomic resolution which is due to a miscut of the YSZ(111) in accordance with αM = 0.67° measured by HRXRD. This can explain the origin of the recorded misalignment for M2(YbFO/BaM/YSZ).
In order to investigate the quality of the individual layers in the heterostructures M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ), we compare the angular diffraction profiles of the BaM0014 and Yb006 reflections for M1 and M2 in Figure 2a,b, respectively. We found that the angular diffraction profile of the (0014) BaM reflection is broader for M1(BaM/YbFO/YSZ), which indicates that the defect density is probably higher in the BaM layer of the M1(BaM/YbFO/YSZ) heterostructure. We applied the mosaic model to the BaM and YbFO layers where the individual layers are composed of mosaic blocks misoriented due to defect formation. The variation in the FWHMang broadening determined for the BaM and YbFO reflections is plotted as a function of the reflection order 00l in Figure 2c,d, respectively. By applying the Williamson–Hall approach [52] for the FWHMang versus 00l plot, we derived the degree of misorientation of the BaM mosaic blocks from the slope. We found that αBaM_M1 = 0.74° is higher than αBaM_M2 = 0.41°, which confirms a higher defect density in the BaM layer of M1 in comparison to the BaM layer of M2. The cross-section TEM images of M1 and M2 in Figure 2e,f indicate a higher number of defect boundaries which are illustrated by yellow dashed curves for the BaM layers. The lateral sizes of BaM mosaic blocks vary in the range from 29 to 154 nm for M1 and in the range between 46 and 169 nm in the case of M2. The X-ray diffraction analysis in combination with TEM characterization enabled us to conclude that the BaM layer in M1 contains more defect boundaries than in the case of M2. However, a similar approach applied to the YbFO layers demonstrated similarities in the quality of the YbFO layer for both heterostructures despite the degree of misorientation being slightly different (αYbFO_M1 = 0.64° and αYbFO_M2 = 0.53°). Figure 3a,h show HRTEM micrographs of the M1 and M2 multiferroic systems, which include the different orientations of the different individual layers such as YSZ, YbFO, and BaM. For both M1 and M2 bilayer systems, BaM and YbFO were grown with the [001] direction parallel to the [111] direction of YSZ. A high-resolution STEM HAADF image of the YbFO/YSZ(111) interface in the M1 heterostructure is given in Figure S2a where an interlayer with a thickness of Th = 2.5 nm and a different atomic arrangement can be seen that in addition exhibits a different image contrast than in the YbFO layer. Furthermore, there were no detectable atomic steps at the YbFO/YSZ(111) interface.
The YbFO layer in the M2(YbFO/BaM/YSZ) heterostructure shows a different interface with the BaM layer. The high-resolution STEM HAADF imaging of the YbFO/BaM interface (Figure S2d) demonstrates the existence of well-resolved atomic steps at the YbFO(AFM)/BaM(FM) interface. It should be emphasized that the lattice misfit is reduced from fM1YbFO/YSZ = −4.42% in M1 to fM2YbFO/BaM = 0.35% in M2. The diffractograms in Figure 3c,e correspond to the YbFO regions marked with dashed green and orange squares in Figure 3a,h, respectively. Different diffraction spots are visible for M1 and M2 due to the different in-plane crystallographic orientation of the YbFO layers. We found that the in-plane orientation of the YbFO layer changes from [2-1-10] in M1 to [10-10] in M2. This indicates that YbFO grown on BaM(001) in M2 is rotated by 30° (±60°) around the [001] direction compared to the YbFO layer grown on YSZ(111) in M1 (cf. Figure 3c,e).
In a similar way, we compared the crystal structure and orientation of the BaM layers in M1 and M2 based on the diffractograms in Figure 3b,d. It turns out that the in-plane orientation of the BaM layer is not affected by the growth sequence.
However, the sharpness and the quality of the interface of BaM to YbFO in M1 and to YSZ in M2 are different. The TEM micrographs of M1 indicate a sharp interface between BaM and YbFO because of the low value of the lattice misfit fM1BaM/YbFO which is about −3.56%, while the BaM in the M2 system forms an interlayer when it grows directly on the YSZ(111) substrate. The nature of the interlayer will be discussed in detail in the following chapter.
The measured XRR curves of M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) together with the fits are given in Figure 4a. The variation in the mass densities ρ with penetration depth is plotted for M1 (black solid line) and M2 (red solid line) in Figure 4b, where the thickness Th = 0 nm corresponds to the surface of the heterostructures. In Figure 4b, we assume that the mass densities of the substrate YSZ as well as of the YbFO and BaM layers are constant as they are limited by short dashed vertical lines. Furthermore, the mass densities of the targets BaFe12O19, YbFeO3, and YSZ(111) are given by ρBaFe12O19 = 5.296 g/cm3, ρ YbFeO3 = 6.8 g/cm3, and ρYSZ = 5.92 g/cm3, respectively, and are drawn by the horizontal gray dashed lines in Figure 4b. The transition regions which correspond to the interfaces with the YSZ(111) substrate (i.e., BaM/YSZ for M2 and YbFO/YSZ for M1) and between the bilayers (BaM/YbFO for M1 and YbFO/BaM for M2) are highlighted by green and gray rectangles to be investigated with higher magnification for the thickness x-axis scale in Figure 4c. The latter was devoted to clearly visualize the changes at the interface and to measure the dimensions of the transition regions at the mentioned interfaces in the heterostructures where the mass density varies with the thickness Th. The extension of the transition regions at the interfaces was estimated from the mass density profiles for M1 and M2 and are summarized in Table 2. For M1, the transition regions RM1Tr1 and RM1Tr2 (respectively RM2Tr1 and RM2Tr2 for M2) correspond to the interface at the substrate and between the individual layers.
The interface near the YSZ(111) substrate for M1 RM1Tr1 = 2.81 ± 0.1 nm is smaller than the RM2Tr1 = 3.95 ± 0.1 nm of M2 as illustrated by green boxes in the right panel of Figure 4c. This indicates that the interface with the substrate is sharper in the case of M1. However, for both heterostructures M1 and M2, the mass density ρ of the layer which is deposited on YSZ(111) (YbFO for M1, BaM for M2) deviates from the one of the used target. This can be due to interdiffusion phenomena of substrate atoms into the grown layer. The chemical composition variation across the heterostructures is displayed in Figure 5 and Figure 6.
The left panel of Figure 4c compares the behavior of the transition regions RM1Tr2 and RM2Tr2 of the interfaces BaM/YbFO for M1 and YbFO/BaM for M2. We found that RM2Tr2 = 10.3 ± 0.1 nm is larger than RM1Tr2 = 8.2 ± 0.1 nm. This suggests the formation of a more distinguished interface BaM/YbFO for M1. Additionally, the mass density of YbFO slightly deviates from the one of the sputtered target YbFeO3. For M2, the BaM layer fits well with the stoichiometry of the BaFe12O19 target as demonstrated from the mass density profile which merges with ρBaM.
In Figure 5a,j, high-resolution STEM HAADF images are given of the YbFO layer grown on YSZ(111) for M1(BaM/YbFO/YSZ) and BaM directly deposited on YSZ(111) for M2(YbFO/BaM/YSZ), where, in the rectangular regions marked by white boxes, combined STEM/EDXS analyses were performed. The corresponding STEM HAADF images and quantified X-ray maps for the elements Ba, Fe, Yb, Zr, and O are shown in Figure 5d–h for M1 and Figure 5m–r for M2. The obtained element-specific line profiles of M1 and M2 are given in Figure 5i,r. Figure 5i displays the profiles of Ba, Fe, Yb, Zr, and O for the heterostructure M1 in a region near the YbFO/YSZ interface, limited by the white box and crossing through the interface which is illustrated by the dashed magenta lines in Figure 5a. The latter contains a disturbed structure where a different atomic arrangement appears as a mixture between the pure YbFO layer and the pure YSZ substrate. Here, from the STEM HAADF image in Figure 5d and from the EDXS maps (Figure 5e–h) and the corresponding elemental profiles, we can distinguish four characteristic ranges RM1YSZ, RM1int1, RM1int2, and RM1YbFO. The region RM1YSZ = Th < 2.75 nm represents the pure substrate YSZ(111), while the region RM1YbFO = Th > 4.6 nm corresponds to a pure YbFO layer of M1 with corresponding slight concentration oscillations of Yb, Fe, and O. The transition region comprises RM1int1 = 2.75 nm < Th < 4.6 nm, where the interdiffusion of Zr into the YbFO layer took place as measured by the simultaneous increase in Yb and Fe and decrease in Zr. Another region, RM1int2 = 4.6 nm < Th < 6.5 nm, defines the deposited YbFeO film in M1 near the interface with residual Zr atoms from the substrate, which are not detected at Th = 6.5 nm away from the YSZ substrate. Therefore, the element concentration profile in RM1int1 has the same behavior as in RM1YSZ with a progressive decrease in the Zr concentration, while RM1int2 displays similar elements with a residual concentration of Zr.
In summary, the interlayer corresponds to a transition region with a thickness of about Th ≅ 4 nm RM1tr = RM1int1 + RM1int2 = 2.75 < Th < 6.5 nm. The evaluation of the mass density profiles for M1 from the XRR fitting gives a transition region between the mass densities of YSZ and YbFO with a thickness of Th = 2.3 nm, which mostly reflects the size of RM1int1 = 2.75 nm < Th < 4.6 nm determined from the Zr and Yb elemental profiles.
Figure 5b,c depict the diffractograms of the YbFO and YSZ(111) substrates indicating the growth of a highly c-axis-oriented YbFO layer, despite the presence of the interdiffusion region.
From the STEM HAADF image contrast visible in Figure 5j,m, it can be clearly seen that the interfacial region between BaM and YSZ indicated by white dashed lines appears to be relatively diffuse. For M2, four defined regions RM1YSZ, RM2int1, RM2int2, and RM2BaM are found in the corresponding Ba, Fe, Yb, Zr, and O element profiles. The transition region RM2tr in the heterostructure M2 corresponds to RM2int1 + RM2int2 where RM2int1 = 1.25 nm < Th < 2.9 nm shows an intermixing between the elements of the substrate (i.e., Zr) and those of the BaM layer (i.e., Ba, Fe). Furthermore, in the second part of the transition region RM2int2 = 2.9 nm < Th < 4.8 nm, the Zr and O concentrations χ [at%] decrease, while the concentrations of Fe and Ba increase. This behavior suggests that the chemical composition of the interlayer regions RM2int1 and RM2int2 do not follow either the structure of the substrate or the one of the BaM top layer. This results in the formation of the transition region RM2tr with a thickness of about Th ≅ 3.55 nm between the YSZ substrate and the BaM layer in the system M2. Furthermore, the regions RM2YSZ and RM2BaM correspond to the pure substrate and the BaM layer in the M2 heterostructure, respectively. The high-resolution STEM image in Figure S2b depicts different regions at the BaM/YSZ interface for M2, where the transition region RM2tr with a disturbed crystal structure and an accordingly diffuse image contrast extends over a thickness of Th = 4.6 to 6.7 nm across the interface. This finding is in accordance with the size of the transition region of the mass density profile measured by XRR at the BaM/YSZ for M2 and estimated to be about Th = 4.3 nm (see Figure 4c). Furthermore, M2 also contains few regions where the BaM/YSZ interface does exhibit a chemical intermixing, as shown in Figure S2c.
The study of the interface chemistry near to the YSZ(111) substrate in both heterostructures M1 and M2 demonstrates the formation of a region with chemical intermixing over a thickness of about Th = 3.5 to 4 nm, which comprises the elements of the substrate and YbFO in M1, resp. BaM in M2.
Figure 5k,l show the diffractograms of the BaM and the interlayer RM2int2. It was not possible to record the inclination angle β = 0.1°, which is visible in the 2D-HRXRD reciprocal space map of Figure 1g. Furthermore, the diffractogram of Figure 5l which corresponds to RM2int2 indicates the existence of crystalline phases, and the elemental profile reveals that these phases are rich in Fe and contain Ba as an impurity (see Figure 5r).
Figure 6a–g show the structure and chemical composition of the YbFO/BaM interfacial region in M2. For this purpose, we recorded large-scale X-ray maps (not shown here) corresponding to the STEM HAADF image in Figure 6a, and the derived element profiles are presented in Figure 6g. It should be noted that because of the large field of view of the scanned area in Figure 6a, the image resolution is relatively poor, and hence, single atomic columns are not resolved. However, we also provided atomically resolved STEM HAADF images and EDXS maps as shown in Figure 6b–f, which correspond to the region marked with a white box in Figure 6a. Generally, from the Ba, Fe, Yb, and O element profiles (see Figure 6g), we can distinguish three important regions, RM2BaM, RM2int3, and RM2YbFO, which are also indicated in the STEM image of Figure 6a. In Figure 6g, the regions RM2BaM and RM2YbFO are defined as regions of constant Ba and Yb concentrations χ, respectively, while RM2int3 represents the transition region around the YbFO/BaM interface in M2, where a chemical intermixing is detected over an estimated extension across the interface of RM2int3 = 9.11 ± 0.05 nm (cf. Table 2b). In addition, Figure 6g contains as an inset element profiles taken with atomic resolution that partially detect the interdiffusion of Ba atoms into the YbFO layer. The region RM2int3 = 9.11 ± 0.05 nm measured from the EDXS profiles was found to be comparable with RM2Tr2 = 10.3 ± 0.05 nm measured in the mass density profiles ρ derived from the XRR fitting procedure in the right panel of Figure 4c. Furthermore, the high-resolution STEM HAADF image of Figure S2d shows an atomic step at the interface YbFO/BaM for M2. The structure and chemical composition of the M1 heterostructure were also explored at atomic resolution in a region near the BaM/YbFO interface for comparison with M2. Figure 6h depicts an atomically resolved STEM HAADF image of M1(BaM/YbFO/YSZ) in a region near the YbFO/BaM interface. From the region marked with an orange rectangle, X-ray maps were recorded and subsequently quantified (see Figure 6i–m). The resulting element concentration profiles of Ba, Yb, Fe, and O are compared in Figure 6n. Here, three characteristic regions, RM1YbFO, RM1BaM, and RM1int3, can be defined. RM1int3 = 2.5 ± 0.05 nm = 4.5 < Th < 7 nm corresponds to the chemical transition region at the YbFO/BaM interface. The latter is found to be significantly reduced in comparison with RM2int3 = 9.11 ± 0.05 nm and does not reveal any chemical intermixture between BaM and YbFO of the M1 bilayers as it can be deduced from the element profiles of Figure 6n. It should be mentioned that the transition region RM2Tr2 = 8.2 ± 0.1 nm as determined from mass density (cf. Figure 4c) is relatively larger than RM2int3 = 2.5 ± 0.05 nm measured from the element profiles (see Table 2b). From our EDXS investigation, we conclude that the degree of Yb/Ba intermixing depends on the stacking sequence. In fact, a relatively abrupt BaM/YbFO interface was detected in M1, while the YbFO/BaM interface in M2 appeared to be more chemically intermixed. Moreover, independently of the growth sequence, an atomic step at the YbFO/BaM and BaM/YbFO interfaces was revealed in M2 and M1, respectively, by atomically resolved STEM imaging, as depicted in Figure S2d,e for both heterostructures, which could induce a magnetic frustration as reported by Chen et al. [53]. Regarding the crystal structure of the BaM and YbFO layers, the number of defect boundaries and the degree of misorientation of the BaM mosaic blocks were found to be affected by the stacking order of the layers (see Figure 2).
Figure S3a,d show atomically resolved STEM HAADF images of the YbFO layers for the M1 and M2 heterostructures in areas of 12 nm × 12 nm. The diffractograms obtained by FFT analysis of the selected red and yellow square regions within the YbFO layers of M1 and M2 are shown in Figure S3b and S3c, respectively. The diffractograms confirm that the growth sequence does not affect the ferroelectric metaphase of YbFeO3, which belongs to space group P63cm. Figure S3a,d illustrate the atomic arrangement of the YbFO layer with representatively colored spheres. Green and yellow spheres represent Yb atoms, appearing with bright contrast in STEM HAADF images (green spheres displaced upwards and yellow spheres displaced downwards), while brown spheres represent Fe atoms with a darker HAADF contrast. As a result, and independently of the stacking order of the YbFO layer, ferroelectric domains were imaged for M1 and M2. In these domains, a non-centrosymmetric shift of Yb atoms generates charge polarization. Specifically, two Yb atoms are shifted vertically upwards, while one is shifted downwards which results in a ferroelectric polarization in the upward direction. Furthermore, Figure S3d reveals a stacking fault (SF), which had formed by the absence of Yb atoms and the successive stacking of two Fe layers. This effect was only detected in a specific imaged region.

3.2. Effect of Growth Sequence on the Magnetic Properties

The out-of-plane (OOP) hysteresis loops recorded for the temperature range T = [50–400 K] for M1 and M2 are compared in Figure 7a, while the in-plane (IP) hysteresis loops are displayed in Figure 7b. The latter shows a higher IP area for the hysteresis loops in M1. Moreover, the IP coercivities and the remenance of M1 are higher than in the case of M2. Similarly, for the whole temperature range, we found that the OOP area, which corresponds to the dissipation energy, is large in the case of M1. One can deduce that the growth sequence changes the hard magnet M1(BaM/YbFO/YSZ) into a soft one M2(YbFO/BaM/YSZ) with a smaller area of the hysteresis loop (i.e., smaller hysteresis loss) and a lower coercivity field Hc. Furthermore, independently of the stacking sequence, the OOP hysteresis loops display single magnetic hysteresis curves rather than the step-like hysteresis loop for the whole measured temperature range T = [50–400 K]. This is in accordance with the abrupt interface BaM/YbFO in M1(BaM/YbFO/YSZ) (Figure 6n) and the slightly intermixed interface YbFO/BaM in the case of M2(YbFO/BaM/YSZ) (Figure 6g). For better clarity, in Figure 7c, the OOP of the heterostructures M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) are compared for T = 50 and 300 K. In order to investigate the existence of interfacial magnetic coupling (EB) below the Neel temperature of YbFeO3 (TN ≅ 125 K) [16,17,19] for M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ), field-cooled hysteresis loops were measured after cooling to 50 K below the Neel temperature of the YbFO layer (i.e., TYbFON ≅ 140 K) under a field of +2 T and −2 T. The results given in Figure 7d do not show any detectable exchange bias (EB) for the M1 and M2 heterostructures at T = 50 K where the systems M1 and M2 correspond to (FM/CAFM) and (CAFM/FM), respectively. We did not consider to perform the EB measurement since the Neel temperature of YbFO was TYbFON ≅ 140 K, and the systems M1 and M2 underwent a transition to (FM/PM) and (PM/FM), respectively, where the EB was not relevant.
The EDXS profiles of M2(YbFO/BaM/YSZ) demonstrate a chemical intermixture between Yb and Ba cations over an intermixed region of RM2int3 = 8.7 ± 0.05 nm at the YbFO/BaM interface (Figure 6g, Table 2).
The chemical profile played a significant role in the magnetic coupling across the interface for other FM/AFM M1(BaM/YbFO/YSZ) and AFM/FM M2(YbFO/BaM/YSZ) heterostructures. It was found by Chen et al. [33] that a strong chemical intermixture between Mn3+ and Fe3+ generated an EB in the magnetization loops for LaMnO3/LaFeO3 due to uncompensated spins at the surface of the antiferromagnetic layer. Despite the presence of the intermixed region between the Yb and Ba atoms in the case of M2(YbFO/BaM/YSZ) at the interface YbFO/BaM, it seems that the spins of the YbFO layer at the interface were completely compensated. They energetically favored the spin flopping configuration which did not induce the EB in Figure 7d as has been recorded in the M1 and M2 heterostructures. Furthermore, several studies [32,33,34] confirmed the absence of an EB in the case of chemically abrupt interfaces similar to the one revealed in the case of M1(BaM/YbFO/YSZ). It is worthwhile emphasizing that YbFO is known by its canted antiferromagnetic spin orientations. This will strongly influence the spin ordering in the vicinity of the interface and remarkably contribute to the spin-flop phase as reported by Jensen et al. [37].
In order to understand and to compare the temperature dependence of magnetic properties for M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ), the values of Ms(T), Hc(T), and Ha(T) are derived from Figure 7 and plotted with the temperature in Figure 8. The analysis procedure of the (IP) and (OOP) curves is explained above in Section 3.2.
The Curie temperature TFSc of the BaM single crystal in the free-standing state was previously determined by Shirk et al. at Tc = 740 K [54]. In our case, the stacking sequence changed the in-plane residual strain in the BaM layer from compressive εM1BaM// = −1.3% in M1 to tensile in M2 εM2BaM// = 1.3%, while the out-of-plane residual strain increased from εM1BaM⊥ = 0.29% to εM2BaM⊥ = 0.48% (see Table 1c). The Tc was determined for M1 and M2 from the derivatives minimum dM/dT of the temperature–moment dependence M//(T) curve (see Figure 8a). We found TM1c = 723.5 ± 5 K and TM2c = 714.7 ± 5 K for the BaM layer in M1 and M2 which was lower than Tc = 740 K for BaM in the free-standing state. The lowering of the Tc of the strained film in comparison to the bulk has been also reported by Gan et al. in the case of epitaxial SrRuO3 films [28].
It is well known that the anisotropy constant K1(T) is related to the anisotropy field Ha(T) and to the Ms(T) and can be estimated from Equation (1) as follows [54,55,56,57,58]:
K 1 ( T ) = M s   ( T ) × H a   ( T ) 2
Here, Ha(T) was obtained from the intersection obtained by extrapolating the linear part of a (IP) hysteretic magnetization curve to saturation, while the saturation magnetization level Ms(T) was determined from the (OOP) curves recorded at different temperatures T between 50 K and 400 K. As a result, the temperature dependences of Ms(T) and K1(T) are given in Figure 8b,c. The decrease in Ms⊥(T) by increasing T for the M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) heterostructures is due to the breaking of the spin ordering. Furthermore, Ms⊥ (T) is lower in M2 than in M1, and this can be explained by an intermixed range RM2int3 = 8.7 ± 0.05 nm.
The anisotropy constant K1(T) also defines the magneto-crystalline anisotropy energy (MAE) which decreases with T due to the weakening of the spin orbital coupling (SOC) because of the thermal fluctuation. However, the values of K1(T) are found to be higher for M1(BaM/YbFO/YSZ) (see Figure 8c). This indicates that the SOC is influenced by the stacking sequence and is strong in the case of M1(BaM/YbFO/YSZ) which is more suitable for magnetic storage devices. The high values of K1(T) are in accordance with high c-axis orientation as revealed for M1(BaM/YbFO/YSZ) in contrast to M2(YbFO/BaM/YSZ), where the c-axis orientation of the heterostructures is off-axis with an inclination angle β = 0.1° with respect to the normal of the YSZ(111) lattice planes (see Figure 1f,g).
In order to compare the temperature-dependent saturation magnetization Ms(T) and first-order anisotropy constant K1(T) between M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ), both Ms(T) and K1(T) were fitted by the modified Bloch’s law [57] as a power law, which is given by the following equations Equations (2) and (3) [56]. It has been demonstrated that the well-known Bloch’s T3/2 law, which is derived from the spin-wave theory of the thermal excitation of magnons, cannot fully describe Ms(T) for complex magnetic structures such as the hexaferrite [57,59].
M s   ( T ) = M s   ( 0 ) × [ 1 ( T T c ) P ]
K 1   ( T ) = K 1   ( 0 ) × [ 1 ( T T c ) P ]
(Ms(0), P) and (K1(0), P) are the fitting parameters derived from the best fit of Ms (T) and K1(T), respectively, by using the non-linear square fit algorithms with chi-square values R = 0.999, which are shown in Figure 8b,c. The exponent P depends on the dimensionality, predominant spin, and crystal structure. In the case of homogeneous ferromagnetic materials, we apply P = 3/2 in Bloch’s law. It should be noted that TM1c = 723.5 ± 5 K and TM2c = 730.6 ± 5 K are used as fixed parameters as they were previously derived from Figure 8a.
The temperature dependence of the first anisotropy constant K1 and saturation magnetization Ms also obeyed the power law with the exponents P = 1.58 ± 0.04 and P = 1.56 ± 0.11, respectively, for silica-coated BaFe12O19 nanoparticles [56]. In the case of M1 and M2 heterostructures, Ms⊥(T) and K1(T) deviated from Bloch’s T3/2 law, which was applicable for example, to BaFe12O19 nanoparticles. The exponents derived from Ms⊥(T) were PM1Ms⊥= 1.277 ± 0.040 and PM2Ms⊥=1.253 ± 0.037 which were comparable for M1 and M2 in the range of uncertainty. On the other hand, the exponents derived from K1(T) were different from those derived from Ms⊥ (T). In fact, for M1, the exponent was PM1K1=1.432 ± 0.060, while for M2, it was PM2K1 = 1.861 ± 0.093 (see Table 3). As result, the difference between PM1Ms⊥ and PM1K1 for M1 was found to be smaller than the recorded the difference between the PM2Ms⊥ and PM2K1 values for M2. This can be related to the better homogeneity of M1 in comparison with M2, which exhibited a region of the chemical intermixing RM2int3 = 8.7 ± 0.05 nm at the BaM/YbFO interface, affecting the resulting magnetic properties of the heterostructure M2. Similar phenomena were revealed by Garcia et al. who reported significant higher values for the exponents P in the case of yttrium iron garnets doped with Zn, Ni, and Co due to the atomic disorder and magnetic frustrations [59].
In order to explain the mechanism controlling the enhancement of the coercivity field and to understand the influence of the growth sequence on the temperature dependence Hc(T), we use the following relation which is based on the micromagnetic model [58,60,61,62,63]:
H c   ( T ) M s   ( T ) = α × H a   ( T ) M s   ( T ) N e f f ,
where N e f f is the demagnetization factor resulting from grain surface and volume charges, and α corresponds to a microstructural parameter which is also called the structural reduction factor [58]. The latter α = α1 × α2 is defined by Kronmüller et al. [58] as a product of α1 which is the pinning or the nucleation factor, and α2 is related to the misalignment factor of the grains with respect to the c-axis.
The plot H c   ( T ) M s   ( T ) versus H a   ( T ) M s   ( T ) in Figure 8d enables us to determine the structural reduction factors αM1 = 0.116 and αM2 = 0.04 from the slopes which are lower than α = 0.5, and this indicates that the mechanism which controls the coercivity is mixed. This includes the nucleation and the domain wall [58,60]. Since the misalignment with respect to c-axis is β = 0.1° for M2 and β = 0.01° for M1, as determined from 2D-HRXRD (Figure 1f,g), the factor αM22 is probably higher than αM12. In this case, the high value of αM1 = 0.116 with respect to αM2 = 0.04 can be interpreted by the high number of pinning and nucleation centers which are located at mosaic boundaries which are increased in the case of the M1 heterostructure (see Figure 2e). This in turn explains the increase in the coercivity HcM1⊥(T) values for M1 in comparison with M2, which contains fewer mosaic boundaries and therefore fewer pinning centers (Figure 8e). Moreover, the demagnetization factors NM1eff = 0.072 and NM2eff = −0.003, which were derived from the intercept of the y-axis, are relatively small (see Table 3). This can be interpreted by the reduced number of nonmagnetic phases in both heterostructures as demonstrated by Kronmüller et al. [58]. Nevertheless, this demagnetization factor NM1eff is higher than in M2, indicating a higher defect density in the BaM layer of M1 despite the selectivity of the BaM/YbFO interface. The demagnetization factor Neff was demonstrated to decrease with the grain misalignment and to be inversely proportional to the lateral size of the mosaic blocks [61]. This corresponds to the case of M2 where the misalignment βM2 = 0.1 and βM1 = 0.01 (Figure 1h,k) and the lateral size of the mosaic blocks is larger than in M1 (Figure 2e,f).
Figure S4a presents the initial magnetization curves (IMC) of the M1 and M2 heterostructures, which were measured at T = 300 K to investigate domain wall motion and to determine the susceptibility of these systems. The inset in Figure S4a provides a magnified view corresponding to magnetic fields below 5000 Oe. The curves of M1 and M2 exhibit a two-slope behavior, suggesting the potential existence of two distinct domain wall motion mechanisms. The first slopes are defined by the dashed lines as the tangent of the curves for the magnetic field up to approximately 1000 Oe. The latter are related with the predominant mechanism of domain wall pinning. For M1 and M2, beyond the field of 1000 Oe, the slope of the IMC changes and becomes steeper compared to the initial slope (<1000 Oe) as clearly shown in the inset of Figure S4a. The critical coercivity Hcrit is defined as the field which corresponds to the change in the slopes in the IMC of M1 and M2. For the applied magnetic field below 1000 Oe, there is high material resistance which hinders the domain wall motion. On the contrary, beyond the magnetic field of 1000 Oe there is an increase in the curve slopes which indicates an overcoming of the resistance and enhancement of the domain wall motion mechanism. Furthermore, comparing the two first slopes of M1 and M2, we deduce that the slope of M1 is smaller than M2 which means the domain wall pinning effect is strong in M1. To determine accurately Hcrit, the second and third derivatives of the IMC (d2M/dH2 and d3M/dH3) were analyzed, as shown in Figure S4b for M1 and Figure S4c for M2. Hcrit is identified at the point where the third derivative equals zero. This marks the change in the slope of the IMC. For M1, HM1crit = 1217 Oe, while for M2, HM2crit = 913 Oe. This finding indicates that the depinning of domains in M1 occurs at a higher external field HM1crit = 1217 Oe, which supports the hypothesis that a higher concentration of defects in a material requires a stronger field for domain wall depinning [64].
Figure 8e shows the temperature dependence of the (OOP) coercivity field Hc(T) (bottom panel) and anisotropy field Ha(T) (top panel) in the temperature range T = [50–400 K]. For both heterostructures M1 and M2, Hc(T) and Ha (T) increase with T; however, the values of Hc(T) and Ha(T) are higher in the case of M1(BaM/YbFO/YSZ) with HM1c = [990 (50 K)–1296 Oe (400 K)] due to the probably high number of mosaic boundaries in the BaM layer as shown by TEM in Figure 2e,f. This in turn plays a role in domain wall pinning and therefore enhances Hc(T) and consequently Ha(T). The temperature dependence Hc(T) and Ha(T) of the BaM hexaferrite was investigated in earlier studies [54,55,57]. The increase in Hc(T) and Ha(T) reached a maximum beyond T = 400 K and below 500 K, followed by a decay toward the Curie temperature Tc = 740 K for the BaM single crystals [54]. In Figure 8f, zero-field cooling (ZFCM1M⊥, ZFCM2M⊥) and field cooling (FCM1M⊥, FCM2M⊥) curves are plotted for M1 and M2 as a function of temperature in the range T = 50–400 K with an applied field of H = 0 and H = 2000 Oe, respectively, where H is parallel to the c-axis. It should be reminded that Happ = 2000 Oe is higher than the coercivity of M1 HM1c = 990 (50 K)–1296 Oe (400 K) and M2 with HM2c = 407 (50 K)–448 Oe (400 K) (see Figure 8e). The high anisotropy constant KM11 recorded for M1 lowered the moment ZFCM1M⊥ at T = 50 K in comparison with ZFCM2M⊥. Moreover, for both heterostructures M1 and M2, a thermal irreversibility (FCM⊥ > ZFCM⊥) was recorded due the magnetic anisotropy [65], but the degree of bifurcation (ZFCM⊥ − FCM⊥) was higher in the case of M2. This can be interpreted as the influence of the magnetic frustration resulting from the intermixed YbFO/BaM interface.

4. Conclusions and Discussion

On two different heterostructures M1 and M2 differing in the stacking of BaM layers as FM and YbFO as canted AFM and FE layers, a detailed study on the structure and the magnetic properties was carried by using complementary analysis methods (i.e., 2D-HRXRD, high-resolution TEM and STEM, atomically resolved EDXS). The difference in the interfacial strain, which was induced by the variation in the growth sequence in M1 and M2, was demonstrated to affect the crystal quality and the chemical composition of the individual BaM and YbFO layers as well as the selectivity and the degree of the chemical homogeneity at the interfaces.
By means of atomic-resolution EDXS, we explored the chemical composition of the interfaces with a YSZ substrate as well as at the BaM/YbFO interface in M1 and YbFO/BaM in M2. Interdiffusion phenomena were detected for M1 and M2 with different chemical compositions at the YSZ substrate interfaces, where a rather Fe-rich crystalline phase was formed at the BaM/YSZ interface in M2. The determined values of the misfit at the YSZ interface in M1 and M2 are comparable and compressive (i.e., fM1YbFO/YSZ = −4.42 [%], fM2BaM/YSZ = −5.53 [%]). The chemical composition of the specific layer that interfaces with the substrate was found to be different from the original stoichiometry of the target as demonstrated by the measurement of the mass densities.
While the interface between BaM and YbFO in M1 was sharp and without any chemical interdiffusion transition over a thickness of RM1int3 = 2.5 ± 0.05 nm, the YbFO/BaM interface in M2 revealed a chemical intermixing over an extension of RM2int3 = 8.7 ± 0.05 nm. This was most probably related to the change in the interfacial misfit from compressive fM1BaM/YbFO = −3.56 [%] to tensile fM2YbFO/BaM = 0.35 [%] strain. For both heterostructures M1 and M2, there was no detectable exchange bias, even in the case of the chemically intermixed interface for the M2 heterostructure.
It should be emphasized that below the Neel temperature of YbFO < TN ≅ 140 K, the heterostructures M1 and M2 acted as FM/CAFM and CAFM/FM, respectively, while in the temperature range beyond TN ≅ 140 K, M1 and M2 were close to FM/PM and PM/FM, respectively. Furthermore, the YbFO layers did not exhibit any variation in the metastable hexagonal p63cm ferroelectric ordering of Yb atoms. Even with varying stress and stacking orders, both systems exhibited the ferroelectric order, which is known as the non-centrosymmetric displacement of the rare earth element (also known as 2up/1down vice versa). The measured magnetic properties of the heterostructures were found to be strongly influenced by the ferromagnetic BaM layer due to the lower magnitude of the YbFO layer moment. The magnetic behavior of M1 and M2 was remarkably related to the crystal quality of the BaM layer which was crucially influenced by its interface properties, including in particular the residual strain, misfit, and chemical homogeneity of the layer and the interfacial region.
For the BaM layers, there was a slight crystallographic misalignment of the layer with respect to the substrate surface in the M2 system. The presence of an interlayer (such as YbFO for M1) was sufficient to suppress the misalignment that originated from the miscut of the substrate crystal resulting from its production. HRXRD, HRTEM, and atomically resolved STEM HAADF imaging confirmed that the BaM layer grown on YSZ had a lower defect concentration because of fewer mosaic boundaries despite the occurrence of an unwanted interlayer formation at the substrate interface.
The temperature dependences of magnetic properties such as Ms, anisotropy constant K1, coercivity Hc, and anisotropy Ha fields were compared between M1 and M2 with the goal to investigate the effect of the growth sequence. As a result, a highly c-axis-orientated BaM layer was obtained in the case of M1, with higher Ha, Ms, and K1 than for BaM in the heterostructure M2.
The extended intermixed region of M2 at the YbFO/BaM interface disturbed the homogeneity of the magnetic layers which induced variable deviations in the values of the exponents derived from Ms(T) and K1(T) in the case of M2 because of the differences in anisotropy (and hence differences in homogeneity).
Furthermore, the intermixing of materials affects the ZFC-FC behavior, where film irregularities result in spin frustration, generating thermal irreversibility and disturbing the regular spin alignment, finally ultimately increasing the degree of bifurcation.
Additionally, it has been proven that tensile stress increases the TC for BaM, while compressive strain suppresses ferromagnetism and reduces the TC. In conclusion, M1 with a distinct interface exhibits more homogeneous magnetic properties without an exchange bias phenomenon. On the other hand, M1 exhibits a larger coercivity, a higher density of defects (mosaic boundaries), a higher anisotropy constant, and a higher MAE. These characteristics suggest that M1 is better suited for magnetic storage applications.

Supplementary Materials

The following supporting information can be downloaded at: https://0-www-mdpi-com.brum.beds.ac.uk/article/10.3390/nano14080711/s1, Figure S1: Inclination of the surface and YSZ crystal lattice in samples (a) M1 and (b) M2. The blue points are the inclination of the surface, the red points the inclination of the crystal lattice of the YSZ substrate, and the green points the difference in the inclinations, e.g., the miscut in the given azimuths. The lines are fits of the experimental data. (c) Reciprocal space maps of YSZ224, YSZ133, BaM-1017, BaM-1018, and YbFO108 of M1 and M2; Figure S2: Additional atomic-resolution HAADF images of the M1 and M2 systems focusing on the following interfaces: (a) YbFO/YSZ interface in the M1 system, highlighting an interlayer with a yellow dashed line, (b) BaM/YSZ interface in the M2 system, where a significant interlayer varying from 4.6 to 6.7 nm is marked by yellow dashed lines along with atomic steps at the BaM interface, (c) BaM/YSZ interface in M2 without an interlayer, with miscut-related YSZ surface steps indicated by a yellow dashed line, (d) YbFO/BaM interface in M2, where interface atomic steps are outlined by a yellow dashed line, and individual atoms are identified by colored filled circles, and (e) BaM/YSZ interface in M1, showcasing surface steps on YbFO with a yellow dashed line and atom identification using colored circles. The scale bars for (a–c) are 5nm and (d–e) are 1 nm in size; Figure S3: High-resolution STEM HAADF images and diffractograms of YbFO layers in M1 and M2 systems. (a,d) HAADF images of YbFO layers in M1 and M2, respectively, illustrating the atomic arrangements with color-coded spheres for Yb (green and yellow) and Fe (brown) atoms. Note a stacking defect in M2 (d). FFT analysis diffractograms of M1 (b) and M2 (c) confirming the ferroelectric metaphase of YbFeO3 in both layers. The scale bars for (a,d) are 2 nm in size; Figure S4: Initial magnetization and Hcrit analysis for M1 and M2 heterostructures (a) initial magnetization curves (IMC) for M1 and M2, with an inset detailing two-slope behavior and determination of Hcrit (highlighted by dashed lines). (b,c) Initial magnetization and its derivatives for M1 and M2, respectively, Hcrit at the zero point of the third derivative, Hcrit is marked by vertical dashed line.

Author Contributions

Conceptualization, S.B.; Software, B.N., X.J., R.S., D.W., C.K., P.M. and L.H.; Investigation, S.B., X.J., R.S., D.W., P.M. and L.H.; Data curation, S.B., B.N., P.M. and L.H.; Writing—original draft, S.B.; Writing—review & editing, S.B., B.N., R.S., C.K., V.H., K.S., T.B. and S.U.; Visualization, B.N.; Supervision, S.B. All authors equally contributed. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the German Research Foundation, grant number SCHN 669/1-1 and BA 1642/8-1. The work was supported by the Czech Science Foundation (project No. 19-10799J) and by the project NanoCent financed by the European Regional Development Fund (ERDF, project No. CZ.02.1.01/0.0/0.0/15.003/0000485) and by Charles University, project GA UK No. 284223.

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

Acknowledgments

The additional funding of this study by the German Research Foundation within the framework of the projects SCHN 669/1-1 and BA 1642/8-1 is also gratefully acknowledged. We acknowledge KIT Light Source for providing the equipment at their beamlines. We also would like to thank the Institute for Beam Physics and Technology (IBPT) for the operation of the storage ring, providing the beam in Karlsruhe Research Acceleration (KARA).

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Chen, D.; Harward, I.; Linderman, K.; Economou, E.; Nie, Y.; Celinski, Z. Properties of ferroelectric/ferromagnetic thin film heterostructures. J. Appl. Phys. 2014, 115, 17D713. [Google Scholar] [CrossRef]
  2. Dun, Y.; Chen, J.; An, D.; Chen, D.; Chen, Y.; Li, Y. Voltage control of millimeter-wave ferromagnetic resonance in multiferroic heterostructures thin films. Phys. Lett. A 2020, 384, 126639. [Google Scholar] [CrossRef]
  3. Bodeux, R.; Michau, D.; Maglione, M.; Josse, M. Thin films sputtered from Ba2NdFeNb4O15 multiferroic targets on BaFe12O19 coated substrates. Mater. Res. Bull. 2016, 81, 49–54. [Google Scholar] [CrossRef]
  4. Hajlaoui, T.; Harnagea, C.; Pignolet, A. Magnetoelectric coupling in room temperature multiferroic Ba2EuFeNb4O15/BaFe12O19 epitaxial heterostructures grown by laser ablation. Nanomaterials 2023, 13, 761. [Google Scholar] [CrossRef]
  5. Srinivasan, G.; Zavislyak, I.V.; Tatarenko, A.S. Millimeter-wave magnetoelectric effects in bilayers of barium hexaferrite and lead zirconate titanate. Appl. Phys. Lett. 2006, 89, 152508. [Google Scholar] [CrossRef]
  6. Srinath, S.; Frey, N.A.; Heindl, R.; Srikanth, H.; Coffey, K.R.; Dudney, N.J. Growth and characterization of sputtered BSTO/BaM multilayers. J. Appl. Phys. 2005, 97, 10J115. [Google Scholar] [CrossRef]
  7. Das, J.; Kalinikos, B.A.; Barman, A.R.; Patton, C.E. Multifunctional dual-tunable low loss ferrite-ferroelctric heterostructures for microwave devices. Appl. Phys. Lett. 2007, 91, 172516. [Google Scholar] [CrossRef]
  8. Das, J.; Song, Y.Y.; Wu, M. Electric-field control of ferromagnetic resonance in monolithic BaFe12O19–Ba0.5Sr0.5TiO3BaFe12O19–Ba0.5Sr0.5TiO3 heterostructures. J. Appl. Phys. 2010, 108, 043911. [Google Scholar] [CrossRef]
  9. Zandalazini, C.I.; Oliva, M.I.; Ferrero, J.C. Structural and magnetic characterization of BaTiO3–BaFe12O19 bilayer thin films: Interface effects on the magnetic properties of barium hexaferrite layer. Ceram. Int. 2021, 47, 19384–19393. [Google Scholar] [CrossRef]
  10. Portugal, R.J.; Peko, J.-C.M.; Hernandes, A.C.; Guaran, C.A.; Guerr, J.D.S. Synthesis and electrical properties of PZT/BaFe12O19 multiferroic ceramics. Key Eng. Mater. 2012, 512, 1291–1295. [Google Scholar] [CrossRef]
  11. Guerra, J.D.S.; Pal, M.; Portugal, R.J.; Cótica, L.F.; Santos, I.A.; Guo, R.; Bhalla, A.S. Multiferroism and magnetoelectric coupling in (PbZr0.65Ti0.35O3)0.97–(BaFe12O19)0.03 ceramic composites. J. Appl. Phys. 2013, 114, 224113. [Google Scholar] [CrossRef]
  12. Guerra, J.D.S.; McIntosh, R.; M’Peko, J.-C.; Hernandes, A.C.; Guo, R.; Bhalla, A.S. Frequency dielectric response of ferroelectric–magnetic ceramic composites like PbZr0.65Ti0.35O3–BaFe12O19. Ceram. Int. 2015, 41, 7091–7096. [Google Scholar] [CrossRef]
  13. Nergis, B.; Bauer, S.; Jin, X.; Seemann, K.; Horak, L.; Schneider, R.; Holy, V.; Ulrich, S.; Baumbach, T. Effect of the laser fluence on the microstructure and the relating magnetic properties of BaFe12O19 films grown on YSZ(111) by PLD for optimized perpendicular recording. J. Mater. Sci. 2023, 58, 718–739. [Google Scholar] [CrossRef]
  14. Bauer, S.; Nergis, B.; Jin, X.; Schneider, R.; Wang, D.; Kübel, C.; Holy, V.; Horak, L.; Seemann, K.; Ulrich, S.; et al. Effect of underlayer quality on microstructure, stoichiometry, and magnetic properties of hexaferrite BaFe12O19 grown on YSZ(111) by PLD. Langmuir 2023, 39, 14308–14327. [Google Scholar] [CrossRef]
  15. Xu, X.; Wang, W. Multiferroic hexagonal ferrites (h-RFeO3, R = Y, Dy-Lu): A brief experimental review. Mod. Phys. Lett. B 2014, 28, 1430008. [Google Scholar] [CrossRef]
  16. Jeong, Y.K.; Lee, J.H.; Ahn, S.J.; Song, S.W.; Jang, H.M.; Choi, H.; Scott, J.F. Structurally tailored hexagonal ferroelectricity and multiferroism in epitaxial YbFeO3 thin-film heterostructures. J. Am. Chem. Soc. 2012, 134, 1450–1453. [Google Scholar] [CrossRef]
  17. Iida, H.; Koizumi, T.; Uesu, Y.; Kohn, K.; Ikeda, N.; Mori, S.; Haumont, R.; Janolin, P.E.; Kiat, J.M.; Fukunaga, M.; et al. Ferroelectricity and ferrimagnetism of hexagonal YbFeO3 thin films. J. Phys. Soc. Jpn. 2012, 81, 024719. [Google Scholar] [CrossRef]
  18. Cao, S.; Sinha, K.; Zhang, X.; Wang, X.; Yin, Y.; N’Diaye, A.T.; Wang, J.; Keavney, D.J.; Paudel, T.R.; Liu, Y.; et al. Electronic structure and direct observation of ferrimagnetism in multiferroic hexagonal YbFeO3. Phys. Rev. B 2017, 95, 224428. [Google Scholar] [CrossRef]
  19. Rai, R.C.; Horvatits, C.; Mckenna, D.; Du Hart, J. Structural studies and physical properties of hexagonal-YbFeO3 thin films. AIP Adv. 2019, 9, 015019. [Google Scholar] [CrossRef]
  20. Xu, X.X.; Yun, Y.; Buragohain, P.; Thind, A.; Yin, Y.; Li, X.; Jiang, X.; Mishra, R.; Gruverman, A. Absence of critical thickness in improper ferroelectric hexagonal-YbFeO3 thin films. Res. Sq. 2020. [Google Scholar] [CrossRef]
  21. Yun, Y.; Buragohain, P.; Thind, A.S.; Yin, Y.; Li, X.; Jiang, X.; Mishra, R.; Gruverman, A.; Xu, X. Spontaneous polarization in an ultrathin improper-ferroelectric/dielectric bilayer in a capacitor structure at cryogenic temperatures. Phys. Rev. Appl. 2022, 18, 034071. [Google Scholar] [CrossRef]
  22. Li, X.; Yun, Y.; Thind, A.S.; Yin, Y.; Li, Q.; Wang, W.; N’Diaye, A.T.; Mellinger, C.; Jiang, X.; Mishra, R.; et al. Domain-wall magnetoelectric coupling in multiferroic hexagonal YbFeO3 films. Sci. Rep. 2023, 13, 1775. [Google Scholar] [CrossRef] [PubMed]
  23. Tikhanova, S.; Seroglazova, A.; Chebanenko, M.; Nevedomskiy, V.; Popkov, V. Effect of TiO2 additives on the stabilization of h-YbFeO3 and promotion of photo-fenton activity of o-YbFeO3/h-YbFeO3/r-TiO2 nanocomposites. Materials 2022, 15, 8273. [Google Scholar] [CrossRef] [PubMed]
  24. Chen, X.; Hua, Z.; Geng, C.; Ma, N. Facile synthesis of novel YbFeO3–BiFeO3 composite for highly sensitive ppb-level acetone sensing at low temperature. J. Mater. Sci. Mater. Electron. 2023, 34, 1588. [Google Scholar] [CrossRef]
  25. Zhang, X.; Yin, Y.; Yang, S.; Yang, Z.; Xu, X. Effect of interface on epitaxy and magnetism in h-RFeO3/Fe3O4/Al2O3 films (R = Lu, Yb). J. Phys. Condens. Matter 2017, 29, 164001. [Google Scholar] [CrossRef] [PubMed]
  26. Fu, Q.; Zhuang, N.; Hu, X.; Chen, J. Substrate influence on the structure and properties of YbFeO3 film. Mater. Res. Express 2019, 6, 126120. [Google Scholar] [CrossRef]
  27. Bibes, M.; Balcells, L.; Valencia, S.; Fontcuberta, J.; Wojcik, M.; Jedryka, E.; Nadolski, S. Nanoscale multiphase separation at La2/3Ca1/3MnO3/SrTiO3 interfaces. Phys. Rev. Lett. 2001, 87, 067210. [Google Scholar] [CrossRef] [PubMed]
  28. Gan, Q.; Rao, R.A.; Eom, C.B.; Garrett, J.L.; Lee, M. Direct measurement of strain effects on magnetic and electrical properties of epitaxial SrRuO3 thin film. Appl. Phys. Lett. 1998, 72, 978. [Google Scholar] [CrossRef]
  29. Vrejoiu, I.; Ziese, M.; Setzer, A.; Esquinazi, P.D.; Birajdar, B.I.; Lotnyk, A.; Alexe, M.; Hesse, D. Interfacial strain effects in epitaxial multiferroic heterostructures of PbZrxTi1−xO3/La0.7Sr0.3MnO3PbZr grown by pulsed-laser deposition. Appl. Phys. Lett. 2008, 92, 152506. [Google Scholar] [CrossRef]
  30. Choi, E.-M.; Sim, K.I.; Burch, K.S.; Lee, Y.H. Emergent multifunctional magnetic proximity in van der Waals layered heterostructures. Adv. Sci. 2022, 9, 2200186. [Google Scholar] [CrossRef]
  31. Huang, H.; Zhai, X.; Wang, J.; Meng, D.; Yun, Y.; Ma, C.; Zheng, X.; Wu, L.; Pan, H.; Fu, Z.; et al. Effect of interface defects on the magnetoresistance in Bi4Ti3O12/(La, Sr)Mn1−xO3 heterostructures. J. Mater. Sci. 2018, 53, 9627–9634. [Google Scholar] [CrossRef]
  32. Vafaee, M.; Finizio, S.; Deniz, H.; Hesse, D.; Zabel, H.; Jakob, G.; Kläui, M. The effect of interface roughness on exchange bias in La0.7Sr0.3MnO3–BiFeO3 heterostructures. Appl. Phys. Lett. 2016, 108, 072401. [Google Scholar] [CrossRef]
  33. Chen, B.; Gauquelin, N.; Green, R.J.; Verbeeck, J.; Rijnders, G.; Koster, G. Asymmetric cation intermixing, magnetic coupling in LaMnO3/LaFeO3 heterostructures. Front. Phys. 2021, 9, 698154. [Google Scholar] [CrossRef]
  34. Neumann, R.F.; Bahiana, M.; Binggeli, N. Magnetic properties of La0.67Sr0.33MnO3/BiFeO3(001) heterojunctions: Chemically abrupt vs. atomic intermixed interface. Europhys. Lett. 2012, 100, 67002. [Google Scholar] [CrossRef]
  35. Huang, Z.; Ariando; Wang, X.R.; Rusydi, A.; Chen, J.; Yang, H.; Venkatesan, T. Interface engineering and emergent phenomena in oxide heterostructures. Adv. Mater. 2018, 30, 1802439. [Google Scholar] [CrossRef] [PubMed]
  36. Malozemoff, A.P. Random-field model of exchange anisotropy at rough ferromagnetic-antiferromagnetic interfaces. Phys. Rev. B 1987, 35, 3679–3682. [Google Scholar] [CrossRef] [PubMed]
  37. Jensen, P.J.; Dreyssé, H.; Kiwi, M. Magnetic reordering in the vicinity of a ferromagnetic/antiferromagnetic interface. Eur. Phys. J. B 2005, 46, 541–551. [Google Scholar] [CrossRef]
  38. Husain, S.; Harris, I.; Gao, G.; Li, X.; Meisenheimer, P.; Shi, C.; Kavle, P.; Choi, C.H.; Kim, T.Y.; Kang, D.; et al. Low-temperature grapho-epitaxial La-substituted BiFeO3 on metallic perovskite. Nat. Commun. 2024, 15, 479. [Google Scholar] [CrossRef]
  39. Xu, J.; Zhu, K.; Hou, Y. Magnetic Heterostructures: Interface Control to Optimize Magnetic Property and Multifunctionality. ACS Appl. Mater. Interfaces 2020, 12, 36811–36822. [Google Scholar] [CrossRef]
  40. Liu, K.; Zhang, R.; Li, J.; Zhang, S. Atomic-Scale Structural Properties in NiCo2O4/CuFe2O4 Bilayer Heterostructures on (001)-MgAl2O4 Substrate Regulated by Film Thickness. Materials 2024, 17, 871. [Google Scholar] [CrossRef]
  41. Koon, N.C. Calculations of exchange bias in thin films with ferromagnetic/antiferromagnetic interfaces. Phys. Rev. Lett. 1997, 78, 4865–4868. [Google Scholar] [CrossRef]
  42. Folven, E.; Scholl, A.; Young, A.; Retterer, S.T.; Boschker, J.E.; Tybell, T.; Takamura, Y.; Grepstad, J.K. Crossover from spin-flop coupling to collinear spin alignment in antiferromagnetic/ferromagnetic nanostructures. Nano Lett. 2012, 12, 2386–2390. [Google Scholar] [CrossRef] [PubMed]
  43. Schulthess, T.C.; Butler, W.H. Consequences of spin-flop coupling in exchange biased films. Phys. Rev. Lett. 1998, 81, 4516–4519. [Google Scholar] [CrossRef]
  44. Berkowitz, A.E.; Takano, K. Exchange anisotropy—A review. J. Magn. Magn. Mater. 1999, 200, 552–570. [Google Scholar] [CrossRef]
  45. Dong, S.; Yamauchi, K.; Yunoki, S.; Yu, R.; Liang, S.; Moreo, A.; Liu, J.-M.; Picozzi, S.; Dagotto, E. Exchange bias driven by the Dzyaloshinskii-Moriya interaction and ferroelectric polarization at G-type antiferromagnetic perovskite interfaces. Phys. Rev. Lett. 2009, 103, 127201. [Google Scholar] [CrossRef] [PubMed]
  46. Zhang, W.; Krishnan, K.M. Epitaxial exchange-bias systems: From fundamentals to future spin-orbitronics. Mater. Sci. Eng. R 2016, 105, 1–20. [Google Scholar] [CrossRef]
  47. Olsen, F.K.; Hallsteinsen, I.; Arenholz, E.; Tybell, T.; Folven, E. Coexisting spin-flop coupling and exchange bias in LaFeO3/La0.7Sr0.3MnO3 heterostructures. Phys. Rev. B 2019, 99, 134411. [Google Scholar] [CrossRef]
  48. Gibert, M.; Viret, M.; Torres-Pardo, A.; Piamonteze, C.; Zubko, P.; Jaouen, N.; Tonnerre, J.-M.; Mougin, A.; Fowlie, J.; Catalano, S.; et al. Interfacial control of magnetic properties at LaMnO3/LaNiO3 interfaces. Nano Lett. 2015, 15, 7355–7361. [Google Scholar] [CrossRef] [PubMed]
  49. Paratt, L.G. Surface studies of solids by total reflection of X-rays. Phys. Rev. 1954, 95, 359–369. [Google Scholar] [CrossRef]
  50. Cliff, W.; Lorimer, G.W. The quantitative analysis of thin specimens. J. Microsc. 1975, 103, 203. [Google Scholar] [CrossRef]
  51. Zehner, J.; Soldatov, I.; Schneider, S.; Heller, R.; Khojasteh, N.B.; Schiemenz, S.; Fähler, S.; Nielsch, K.; Schäfer, R.; Leistner, K. Voltage-controlled deblocking of magnetization reversal in thin films by tunable domain wall interactions and pinning sites. Adv. Electron. Mater. 2020, 6, 2000406. [Google Scholar] [CrossRef]
  52. Williamson, G.K.; Hall, W.H. X-ray line broadening from filed aluminum and wolfram. Acta Metall. 1953, 1, 22. [Google Scholar] [CrossRef]
  53. Ji, T.Z.; Sun, L.; Miao, B.F.; Millev, Y.T.; Ding, H.F. General nature of the step-induced frustration at ferromagnetic/antiferromagnetic interfaces: Topological origin and quantitative understanding. New J. Phys. 2019, 21, 123045. [Google Scholar]
  54. Shirk, B.T.; Buessem, W.R. Temperature dependence of Ms and K1 of BaFe12O19 and SrFe12O19 single crystals. J. Appl. Phys. 1969, 40, 1294–1296. [Google Scholar] [CrossRef]
  55. Zhang, W.; Peng, B.; Zhang, W.; Zhou, S.; Schmidt, H. Ultra large coercivity in barium ferrite thin films prepared by magnetron sputtering. J. Magn. Magn. Mater. 2010, 322, 1859–1862. [Google Scholar] [CrossRef]
  56. Wang, J.; Zhao, F.; Wu, W.; Zhao, G.M. Unusual temperature dependence of the magnetic anisotropy constant in barium ferrite BaFe12O19. J. Appl. Phys. 2011, 110, 096107. [Google Scholar] [CrossRef]
  57. Singh, H.K.; Mohapatra, P.P.; Sahu, S.; Dobbidi, P. Dielectric and temperature dependent magnetic studies of Al3+ substituted Ba0.4La0.1Sr0.5AlxFe12-xO19 hexaferrite for microwave application. Mater. Sci. Eng. B 2022, 284, 115876. [Google Scholar] [CrossRef]
  58. Kronmüller, H.; Durst, K.D.; Sagawa, M. Analysis of the magnetic hardening mechanism in RE-FeB permanent magnets. J. Magn. Magn. Mater. 1988, 74, 291. [Google Scholar] [CrossRef]
  59. Peña-Garcia, R.; Guerra, Y.; de Souza, F.R.; Gonçalves, L.A.P.; Padrón-Hernández, E. The extended Bloch’s law in yttrium iron garnet doped with Zn, Ni and Co. Phys. E Low-Dimens. Syst. Nanostruct. 2018, 103, 354–360. [Google Scholar] [CrossRef]
  60. Liu, B.-H.; Ding, J.; Dong, Z.-L.; Boothroyd, C.-B.; Yin, J.-H.; Yi, J.-B. Microstructural evolution and its influence on the magnetic properties of CoFe2O4 powders during mechanical milling. Phys. Rev. B 2006, 74, 184427. [Google Scholar] [CrossRef]
  61. Bance, S.; Seebacher, B.; Schrefl, T.; Exl, L.; Winklhofer, M.; Hrkac, G.; Zimanyi, G.; Shoji, T.; Yano, M.; Sakuma, N.; et al. Grain-size dependent demagnetizing factors in permanent magnets. J. Appl. Phys. 2014, 116, 233903. [Google Scholar] [CrossRef]
  62. Kou, X.-C.; Kronmüller, H.; Givord, D.; Rossignol, M.F. Coercivity mechanism of sintered Pr17Fe75B8 and Pr17Fe53B30 permanent magnets. Phys. Rev. B 1994, 50, 3849. [Google Scholar] [CrossRef] [PubMed]
  63. Ma, J.; Zhao, X.; Liu, W.; Li, Y.; Liu, L.; Song, Y.; Xie, Y.; Zhao, X.; Zhang, Z. Coercivity mechanism and magnetization reversal in anisotropic Ce-(Y)-Pr-Fe-B films. Materials 2021, 14, 4680. [Google Scholar] [CrossRef] [PubMed]
  64. Qiu, L.; Zhao, L.; Weng, X.; Shen, L.; Zhao, G.; Wang, F.; Xie, L. A hybrid coercivity mechanism for exchange-coupled nanocomposite permanent magnets. J. Rare Earths 2019, 37, 1030–1033. [Google Scholar] [CrossRef]
  65. Kumar, P.S.A.; Joy, P.A.; Date, S.K. Comparison of the irreversible thermomagnetic behaviour of some ferro- and ferrimagnetic systems. Bull. Mater. Sci. 2000, 23, 97–101. [Google Scholar] [CrossRef]
Figure 1. (a) Diffraction patterns of the heterostructures M1(BaM/YbFO/YSZ) (solid black curve) and M2(YbFO/BaM/YSZ) (solid red curve), substrate peaks are shown with (*) symbol. (b,c) Azimuthal scans of asymmetric reflections BaM(−1018) and YbFO(108) for M1 and M2, respectively. (d,e) Visualization of the in-plane rotation relationship of the atomic layers relating to the crystal structures as it is simulated along the [0001] direction for M1 and M2, respectively. (f,g) 2D-HRXRD reciprocal space maps containing the BaM(0016), YbFO(008), and YSZ(222) diffraction spots. (h,i) Schematic presentation of the heterostructures M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) with two different stacking sequences.
Figure 1. (a) Diffraction patterns of the heterostructures M1(BaM/YbFO/YSZ) (solid black curve) and M2(YbFO/BaM/YSZ) (solid red curve), substrate peaks are shown with (*) symbol. (b,c) Azimuthal scans of asymmetric reflections BaM(−1018) and YbFO(108) for M1 and M2, respectively. (d,e) Visualization of the in-plane rotation relationship of the atomic layers relating to the crystal structures as it is simulated along the [0001] direction for M1 and M2, respectively. (f,g) 2D-HRXRD reciprocal space maps containing the BaM(0016), YbFO(008), and YSZ(222) diffraction spots. (h,i) Schematic presentation of the heterostructures M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) with two different stacking sequences.
Nanomaterials 14 00711 g001
Figure 2. (a,b) Comparison between the M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) heterostructures by the angular diffraction profiles of the BaM0014 and YbFO006 reflections, respectively. (c,d) Comparison of M1 and M2 regarding the variation in the full width half maximum of the corresponding angular broadening FWHMang with the reflection order 00l for the BaM and YbFO layers, respectively. (e,f) TEM cross-section images of the M1 and M2 heterostructures, respectively, indicating the mosaic boundaries with yellow dashed lines.
Figure 2. (a,b) Comparison between the M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) heterostructures by the angular diffraction profiles of the BaM0014 and YbFO006 reflections, respectively. (c,d) Comparison of M1 and M2 regarding the variation in the full width half maximum of the corresponding angular broadening FWHMang with the reflection order 00l for the BaM and YbFO layers, respectively. (e,f) TEM cross-section images of the M1 and M2 heterostructures, respectively, indicating the mosaic boundaries with yellow dashed lines.
Nanomaterials 14 00711 g002
Figure 3. (a,h) HRTEM images of M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) in cross-section with the crystallographic orientation of the individual layers BaM, YbFO, and YSZ. (b,c,f) Diffractograms corresponding to M1(BaM/YbFO/YSZ) of the BaM layer drawn by a red box in (a) of the YbFO layer illustrated by a green box (a) and of the YSZ(111) substrate, respectively. (d,e,g) Diffractograms corresponding to M2(BaM/YbFO/YSZ) of the BaM layer drawn by a blue box in (a) of the YbFO layer illustrated by an orange box (h) and of the YSZ(111) substrate, respectively. Scale bars of (a,h) are in size of 20 nm.
Figure 3. (a,h) HRTEM images of M1(BaM/YbFO/YSZ) and M2(YbFO/BaM/YSZ) in cross-section with the crystallographic orientation of the individual layers BaM, YbFO, and YSZ. (b,c,f) Diffractograms corresponding to M1(BaM/YbFO/YSZ) of the BaM layer drawn by a red box in (a) of the YbFO layer illustrated by a green box (a) and of the YSZ(111) substrate, respectively. (d,e,g) Diffractograms corresponding to M2(BaM/YbFO/YSZ) of the BaM layer drawn by a blue box in (a) of the YbFO layer illustrated by an orange box (h) and of the YSZ(111) substrate, respectively. Scale bars of (a,h) are in size of 20 nm.
Nanomaterials 14 00711 g003
Figure 4. (a) Measured XRR curves (points) and the obtained fits (lines) for M1 (black) and M2 (red). The curves are vertically shifted for better visibility. (b) Density profiles obtained from the fits of M1 (black) and M2 (red). (c) Magnified sections of the interfaces of the density profiles marked with dashed squares in (b). The (c) left panel shows the interface between the layers and the (c) right panel shows the YSZ/first layer interface. The density profiles in (c) are shifted with respect to each other for a better comparison of the interfaces.
Figure 4. (a) Measured XRR curves (points) and the obtained fits (lines) for M1 (black) and M2 (red). The curves are vertically shifted for better visibility. (b) Density profiles obtained from the fits of M1 (black) and M2 (red). (c) Magnified sections of the interfaces of the density profiles marked with dashed squares in (b). The (c) left panel shows the interface between the layers and the (c) right panel shows the YSZ/first layer interface. The density profiles in (c) are shifted with respect to each other for a better comparison of the interfaces.
Nanomaterials 14 00711 g004
Figure 5. (a,j) High-resolution STEM HAADF images near the bilayer interface regions (YbFO/YSZ) and (BaM/YSZ) for the M1 and M2 heterostructures, respectively. (b,c) Diffractograms corresponding to red and yellow rectangles drawn in the BaM layer and YSZ substrate, respectively. (k,l) Diffractograms of the red and yellow rectangles drawn in the BaM layer and YSZ substrate, respectively. The regions marked with white rectangles are the regions selected for the corresponding X-ray maps given in (dh) for M1 and in (mq) for M2. (i,r) Comparison of the quantitative EDXS line profiles of the elements O, Fe, Ba, and Yb for M1 and M2, respectively. Scale bars of (a,j) are 5 nm and of (dh) and (mq) are 2 nm in size.
Figure 5. (a,j) High-resolution STEM HAADF images near the bilayer interface regions (YbFO/YSZ) and (BaM/YSZ) for the M1 and M2 heterostructures, respectively. (b,c) Diffractograms corresponding to red and yellow rectangles drawn in the BaM layer and YSZ substrate, respectively. (k,l) Diffractograms of the red and yellow rectangles drawn in the BaM layer and YSZ substrate, respectively. The regions marked with white rectangles are the regions selected for the corresponding X-ray maps given in (dh) for M1 and in (mq) for M2. (i,r) Comparison of the quantitative EDXS line profiles of the elements O, Fe, Ba, and Yb for M1 and M2, respectively. Scale bars of (a,j) are 5 nm and of (dh) and (mq) are 2 nm in size.
Nanomaterials 14 00711 g005
Figure 6. (a,h) High-resolution STEM HAADF images recorded from regions near the bilayer interface (YbFO/BaM) and (BaM/YbFO) for the M2 and M1 heterostructures, respectively. The regions marked with white and orange rectangles are the regions selected for corresponding X-ray maps given in (cf) for M2 and in (jm) for M1, (g,n) comparison of the quantitative EDXS line profiles of the elements Ba, Yb, for M2 and M1. The inset in (g) shows the magnified EDXS line profile illustrated by dashed square regions and black arrow. Scale bars of (a) are 5 nm, of (h) are 2 nm, and of (bf) and (im) are 1 nm in size.
Figure 6. (a,h) High-resolution STEM HAADF images recorded from regions near the bilayer interface (YbFO/BaM) and (BaM/YbFO) for the M2 and M1 heterostructures, respectively. The regions marked with white and orange rectangles are the regions selected for corresponding X-ray maps given in (cf) for M2 and in (jm) for M1, (g,n) comparison of the quantitative EDXS line profiles of the elements Ba, Yb, for M2 and M1. The inset in (g) shows the magnified EDXS line profile illustrated by dashed square regions and black arrow. Scale bars of (a) are 5 nm, of (h) are 2 nm, and of (bf) and (im) are 1 nm in size.
Nanomaterials 14 00711 g006
Figure 7. (a,b) Out-of-plane (OOP) and in-plane (IP) magnetization polarization curves for M1 (top panel) and M2 (bottom panel), respectively, recorded in the temperature range T = [50–400 K]. (c) Comparison between the OOP magnetization of M1 and M2 at T = 50 K and 300 K with the inset as magnification in the region marked with blue dashed square of H = [−1 T–1 T]. (d) OOP magnetization loop measured at 50 K and for applied magnetic field H = 2 T and −2 T for M1 (top panel) and M2 (bottom panel).
Figure 7. (a,b) Out-of-plane (OOP) and in-plane (IP) magnetization polarization curves for M1 (top panel) and M2 (bottom panel), respectively, recorded in the temperature range T = [50–400 K]. (c) Comparison between the OOP magnetization of M1 and M2 at T = 50 K and 300 K with the inset as magnification in the region marked with blue dashed square of H = [−1 T–1 T]. (d) OOP magnetization loop measured at 50 K and for applied magnetic field H = 2 T and −2 T for M1 (top panel) and M2 (bottom panel).
Nanomaterials 14 00711 g007
Figure 8. (a) Variation in the in-plane moment M// versus temperature in the range T = [300–1000 K] for M1 and M2, and inset corresponds to the derivative dM/dT as function of temperature, the minima correspond to the Curie temperature TC. (b) Variation in the out-of-plane moment at the saturation Ms with the temperature for M1 (black full circle) and M2 (red full circle), and the fitting curves are the power law curves. (c) Temperature dependence of the fist anisotropy constant K1 for M1 (black full circle) and M2 (red full circle). (d) Variation in Hc/Ms as function of the Ha/Ms (black full circle) and M2 (red full circle) dedicated to determine microstructural and demagnetizing factors α and Neff, respectively. (e) Anisotropy field Ha temperature dependence (top panel) for M1 and M2 and comparison between M1 and M2 of dependence of perpendicular coercivity Hc with temperature (bottom panel). (f) Zero-field cooling (ZFC) and field cooling (FC) recorded with applied field H = 2000 Oe for M1 (open circles) and M2 (solid lines).
Figure 8. (a) Variation in the in-plane moment M// versus temperature in the range T = [300–1000 K] for M1 and M2, and inset corresponds to the derivative dM/dT as function of temperature, the minima correspond to the Curie temperature TC. (b) Variation in the out-of-plane moment at the saturation Ms with the temperature for M1 (black full circle) and M2 (red full circle), and the fitting curves are the power law curves. (c) Temperature dependence of the fist anisotropy constant K1 for M1 (black full circle) and M2 (red full circle). (d) Variation in Hc/Ms as function of the Ha/Ms (black full circle) and M2 (red full circle) dedicated to determine microstructural and demagnetizing factors α and Neff, respectively. (e) Anisotropy field Ha temperature dependence (top panel) for M1 and M2 and comparison between M1 and M2 of dependence of perpendicular coercivity Hc with temperature (bottom panel). (f) Zero-field cooling (ZFC) and field cooling (FC) recorded with applied field H = 2000 Oe for M1 (open circles) and M2 (solid lines).
Nanomaterials 14 00711 g008
Table 1. (a) Summary of the lattice parameters corresponding to the different layers BaM, YbFO, and YSZ of the heterostructures M1 and M2. (b) Summary of the lattice misfit determined at different interfaces BaM/YbFO, YbFO/YSZ for M1 and YbFO/BaM, BaM/YSZ for M2. (c) Summary of the in-plane and out-of-plane residuals determined in the BaM and YbFO layers in the two different heterostructures M1 and M2.
Table 1. (a) Summary of the lattice parameters corresponding to the different layers BaM, YbFO, and YSZ of the heterostructures M1 and M2. (b) Summary of the lattice misfit determined at different interfaces BaM/YbFO, YbFO/YSZ for M1 and YbFO/BaM, BaM/YSZ for M2. (c) Summary of the in-plane and out-of-plane residuals determined in the BaM and YbFO layers in the two different heterostructures M1 and M2.
(a)
d(11-2)YSZ [Å]d(111)YSZ
[Å]
aM1YbFO
[Å]
aM2YbFO
[Å]
cM1YbFO
[Å]
cM2YbFO
[Å]
aM1BaM
[Å]
aM2BaM
[Å]
cM1BaM [Å]cM2BaM [Å]
M12.100
± 0.001
2.969
± 0.001
6.0221
± 0.001
11.693
± 0.001
5.8151
± 0.001
23.25
± 0.001
M22.100
± 0.001
2.969
± 0.001
5.9881
± 0.001
11.7149
± 0.001
5.967 ± 0.001 23.2942 ± 0.001
(b)
fM1YbFO/YSZ [%]fM1BaM/YbFO [%]fM2BaM/YSZ [%]fM2YbFO/BaM [%]
M1−4.42
compressive
−3.56
compressive
M2 −5.30
compressive
0.35
tensile
(c)
εM1YbFO//
[%]
εM1YbFO⊥
[%]
εM1BaM//
[%]
εM1BaM
[%]
εM2BaM//
[%]
εM2BaM
[%]
εM2YbFO//
[%]
εM2YbFO
[%]
M10.96
Tensile
−0.08
Compressive
−1.3
Compressive
0.29
Tensile
M2 1.3
Tensile
0.48
Tensile
0.39
Tensile
0.11
Tensile
Table 2. (a) Summary of the fitting parameters such as mass densities ρBaM of BaM and ρYbFO of YbFO layer derived from the XRR curves of M1 and M2 and the corresponding density profiles across the heterostructures’ films thicknesses. (b) Summary of the characteristics of regions with their corresponding thicknesses of the EDX profiles of the two heterostructures as they are derived from Figures 5 and 6. (c) Summary of the concentration χ [at %] of the Yb, Fe, and Ba derived from the EDX profiles of Figures 5i and 6n for M1 and from EDX profiles of Figures 5r and 6g for M2.
Table 2. (a) Summary of the fitting parameters such as mass densities ρBaM of BaM and ρYbFO of YbFO layer derived from the XRR curves of M1 and M2 and the corresponding density profiles across the heterostructures’ films thicknesses. (b) Summary of the characteristics of regions with their corresponding thicknesses of the EDX profiles of the two heterostructures as they are derived from Figures 5 and 6. (c) Summary of the concentration χ [at %] of the Yb, Fe, and Ba derived from the EDX profiles of Figures 5i and 6n for M1 and from EDX profiles of Figures 5r and 6g for M2.
(a)
BaM thickness
ThBaM [nm]
XRR
YbFO
thickness
ThYbFO [nm]
XRR
Mass density
ρBaM [g/cm3]
XRR
Mass density
ρYbFO [g/cm3]
XRR
Transition region
YbFO/YSZ
RM1Tr1 [nm]
XRR
Transition region
BaM/YbFO
RM1Tr2 [nm]
XRR
Transition region
BaM/YSZ
RM2Tr1 [nm]
XRR
Transition region
YbFO/BaM
RM2Tr2 [nm]
XRR
M161.0 ± 0.258.8 ± 0.25.24 ± 0.05
≅ ρBaFe12O19
= 5.296 g/cm3
8.38 ± 0.05
> ρ YbFeO3
= 6.8 g/cm3
2.81 ± 0.1 8.2 ± 0.1
M270.0 ± 0.265.0 ± 0.23.86 ± 0.05
< ρBaFe12O19
= 5.296 g/cm3
7.14 ± 0.07
slightly >
ρ YbFeO3
= 6.8 g/cm3
3.95 ± 0.1 10.3 ± 0.1
(b)
BaM thickness
ThBaM [nm]
TEM
YbFO
thickness
ThYbFO [nm]
TEM
YbFO/YSZ
RM1int1 [nm]
EDX profiles
YbFO/YSZ
RM1int2 [nm]
EDX profiles
BaM/YbFO
RM1int3 [nm]
EDX profiles
BaM/YSZ
RM2int1 [nm]
EDX profiles
BaM/YSZ
RM2int2 [nm]
EDX profiles
BaM/YbFO
RM2int3 [nm]
EDX profiles
M163 ± 0.253 ± 0.22.75 < Th < 4.6
1.85 ± 0.05 nm
Interdiffusion of Zr atoms
4.6 < Th < 6.5
1.9 ± 0.05 nm
Residual Zr atoms
4.5 < Th < 7
2.5 ± 0.05 nm
Sharp interface without intermixing
M2 67 ± 0.274 ± 0.2 1.25< Th < 2.9
1.65 ± 0.05 nm
Interdiffusion of Zr atoms
2.9 < Th < 4.8
1.9 ± 0.05 nm
Fe rich phase
4.2 < Th < 12.93
8.7 ± 0.05 nm
Chemical intermixing
(c)
BaM thickness
ThBaM [nm]
TEM
YbFO thickness
ThYbFO [nm]
TEM
RM1YbFO.
χ [at %]
RM1BaM
χ [at %]
RM2YbFO.
χ [at %]
RM2BaM
χ [at %]
M163 ± 0.253 ± 0.2χYb (Max)= 30 ± 1
Yb> = 23.57
Fe> = 27.12
(see Figure 5i)
χBaM (Max) = 7 ± 0.5
Ba> = 3.7
Fe> = 54.03
(see Figure 6n)
M2 67 ± 0.274 ± 0.2 χYb (max) = 18 ± 0.5
Large scan
Yb > = 19.85, <χFe> = 17.97
Atomic resolution
Yb > = 13.89, <χFe > = 18.53
χBaM (Max) = 6 ± 0.5
Large scan
Ba > = 3.18, <χFe> = 36.77
Atomic resolution
BaM> = 3.39, <χFe> = 27.1
Table 3. Summary of the characteristic magnetic parameters for M1 and M2 such as moment at saturation T = 0 K, Ms⊥(0) and exponents P, which were derived from the fitting of temperature dependence moment with the power law Ms⊥(0) × (1 − (T/Tc)P) and K1(0) × (1 − (T/Tc)P). Microstructural parameter α and demagnetization factor Neff were derived from Hc/Ms as function of the Ha/Ms.
Table 3. Summary of the characteristic magnetic parameters for M1 and M2 such as moment at saturation T = 0 K, Ms⊥(0) and exponents P, which were derived from the fitting of temperature dependence moment with the power law Ms⊥(0) × (1 − (T/Tc)P) and K1(0) × (1 − (T/Tc)P). Microstructural parameter α and demagnetization factor Neff were derived from Hc/Ms as function of the Ha/Ms.
Moment at Saturation T = 0 K Ms⊥(0) [emu/cc]Exponent PCurie Temperature Tc [K]Anisotropy Constant K1, T = 0
K1(0) [N/m2]
Exponent PMicrostructural Parameter
α
Demagnetization Factor
Neff
M1MsM1⊥(0) = 573.43 ± 5.97PM1Ms⊥ = 1.277
± 0.040
TM1c = 723.5 ± 5 KM11(0) = 3.5E+6
± 4.4E+3
PM1K1 = 1.432
± 0.060
αM1 = 0.116NM1eff = 0.072
M2MsM2⊥(0) = 513.77 ± 5.68PM2Ms⊥ = 1.253
± 0.037
TM2c = 730.6 ± 5KM21(0) = 2.1E+6
± 2.6E+3
PM2K1 = 1.861
± 0.093
αM2 = 0.041NM2eff = −0.0026
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Bauer, S.; Nergis, B.; Jin, X.; Schneider, R.; Wang, D.; Kübel, C.; Machovec, P.; Horak, L.; Holy, V.; Seemann, K.; et al. Dependence of the Structural and Magnetic Properties on the Growth Sequence in Heterostructures Designed by YbFeO3 and BaFe12O19. Nanomaterials 2024, 14, 711. https://0-doi-org.brum.beds.ac.uk/10.3390/nano14080711

AMA Style

Bauer S, Nergis B, Jin X, Schneider R, Wang D, Kübel C, Machovec P, Horak L, Holy V, Seemann K, et al. Dependence of the Structural and Magnetic Properties on the Growth Sequence in Heterostructures Designed by YbFeO3 and BaFe12O19. Nanomaterials. 2024; 14(8):711. https://0-doi-org.brum.beds.ac.uk/10.3390/nano14080711

Chicago/Turabian Style

Bauer, Sondes, Berkin Nergis, Xiaowei Jin, Reinhard Schneider, Di Wang, Christian Kübel, Petr Machovec, Lukas Horak, Vaclav Holy, Klaus Seemann, and et al. 2024. "Dependence of the Structural and Magnetic Properties on the Growth Sequence in Heterostructures Designed by YbFeO3 and BaFe12O19" Nanomaterials 14, no. 8: 711. https://0-doi-org.brum.beds.ac.uk/10.3390/nano14080711

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop